Yellow ink for uv waterless offset printing discs and preparation method thereof
A technology of waterless offset printing and disc yellowing, which is applied in ink, household utensils, applications, etc., can solve the problems of poor anti-staining, rheological properties and ink transfer performance, and achieve excellent ink transfer performance, low production cost, touch good denaturation effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0042] In parts by weight, use a balance to weigh 12 parts of yellow pigment, 30 parts of polyester acrylate, 8 parts of ethoxy ethoxy ethyl acrylate (EOEOEA), 5 parts of 2,4-diethyl Thioxanthone, 5 parts of fumed silica, 1.5 parts of silicone acrylate, 1 part of polyoxyethylene alkylphenol ether, 0.01 part of glyceryl monostearate, 1 part of methacrylic acid Phosphate ester monomer, then mix the above-mentioned raw material components, and pre-disperse them on a glass plate, and then grind them with a three-roll mill until the pigment is evenly dispersed. And the fineness of the ink is tracked and tested until the fineness of the ink reaches about 5 microns, and the grinding is stopped to obtain the finished product.
Embodiment 2
[0044] In parts by weight, weigh 17 parts of yellow pigment, 55 parts of epoxy acrylate and polyether acrylate (the ratio of weight and number of the two is 1:1) to form a prepolymer, 20 parts of A monomer composed of tripropylene glycol dipropylene ester (TPGDA) and dipropylene glycol diacrylate (DPGDA) (the ratio of the two parts by weight is 1:1), 8 parts of 2-hydroxy-2-methyl-1 -Phenyl-1-acetone, 18 parts of kaolin, 2.5 parts of siloxane acrylate, 2 parts of polyoxyethylene fatty alcohol ether, 0.1 part of sucrose ester, 3 parts of silane coupling agent, and then mix the above-mentioned raw material components, And carry out pre-dispersion on a glass plate, and then use a three-roller grinder to grind until the pigment is evenly dispersed. During the grinding process, adjust the gap of the three-roller grinder in time, and track the fineness of the ink until the ink is fine. When the degree reaches about 5 microns, stop grinding to get the finished product.
Embodiment 3
[0046] In parts by weight, take 15 parts of yellow pigment with a balance, 40 parts of prepolymers composed of polyester acrylate and polyurethane acrylate (the ratio of the parts by weight is 1:1), 10 parts Ethoxylated trimethylolpropane triacrylate (EO3-TMPTA) and propoxylated trimethylolpropane triacrylate (PO3-TMPTA) (the ratio of the two parts by weight is 1:1) Composed monomers, 5 parts of 2-ethylhexyl acrylate, 10 parts of talc, 2 parts of silicone acrylate, 1 part of polyoxyethylene-polyoxypropylene block copolymer, 0.03 parts of sorbitan fatty acid, 2 parts Phosphorus methacrylate monomer, then mix the above raw material components, pre-disperse on a glass plate, and then grind with a three-roll mill until the pigment is evenly dispersed. During the grinding process, adjust the rollers of the three-roll mill Gap gap, and track the fineness of the ink until the fineness of the ink reaches about 5 microns, stop grinding, and the finished product is obtained.
PUM
| Property | Measurement | Unit |
|---|---|---|
| surface tension | aaaaa | aaaaa |
| tackiness | aaaaa | aaaaa |