A high-temperature-resistant wear-resistant non-stick pan coating, its preparation method and its non-stick pan

A non-stick pan and high temperature resistant technology, which is applied in the field of preparation, high temperature resistant and wear-resistant non-stick pan coating, which can solve the problems of coating scratches and peeling, risk of food foreign matter, and low strength of non-stick coating on the surface

Active Publication Date: 2018-05-11
NINGBO GRAMMY KITCHENWARE
View PDF6 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, this material also has many shortcomings, especially the health risks it contains are attracting more and more attention
First of all, the surface non-stick coating formed by Teflon coating is not strong enough to cook with a spatula, and even if only silicone spatulas and wooden spatulas are used for cooking, the coating is easy to absorb after a period of use. Scratches and peelings will affect the structure and performance of the product, and cause the risk of foreign matter in the food; secondly, the temperature of the Teflon coating should generally not exceed 250°C, and according to Chinese cooking habits, for many stir-fried dishes, The temperature in the pot is at least between 300 and 500°C, so it is difficult for people to strictly control it when using it, and it is easy to be damaged by high temperature; third, some studies have found that Teflon materials will release ten gases at high temperatures above 400°C. Several harmful gases have a strong irritating effect on the lungs, and an ingredient called perfluorooctanoic acid ammonium (PFOA) must be added in the production process of Teflon, and concerns about its safety have been expressed in many reports

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • A high-temperature-resistant wear-resistant non-stick pan coating, its preparation method and its non-stick pan

Examples

Experimental program
Comparison scheme
Effect test

preparation example Construction

[0018] The invention provides a method for preparing a high-temperature-resistant and wear-resistant non-stick pan coating, which comprises the following steps: 200-300 parts by mass of nickel sulfate, 45-60 parts by mass of sodium citrate, 50-90 parts by mass of ammonium chloride, 60 - 100 parts by mass of sodium sulfite and deionized water are mixed to obtain the first mixed solution; under the action of an external magnetic field, the metal pan substrate is placed in the first mixed solution for electrochemical nickel plating, and the pH value is adjusted to 8.0-10.0, drying, the temperature of the first mixed liquid is 40-60 ° C, the control current is 50-80A; 80-120 parts by mass of polyarylether nitrile ketone, 1-5 parts by mass of silane coupling agent KH792 Mix with 3-8 parts by mass of nano-silicon tetranitride, stir, and obtain mixture A after electron beam pre-irradiation; spray the mixture A on the inner surface of the metal pan base to obtain a high-temperature-res...

Embodiment 1

[0039] (1) The metal pot body is placed in 20 mass parts of sodium silicate, 40 mass parts of potassium hydroxide, 20 mass parts of potassium carbonate, 20 mass parts of citric acid fatty acid glyceride, 1 mass part of ethylenediamine polyoxyethylene polyoxygen Propylene block polyether, 20 parts by mass of sodium sulfate, 2 parts by mass of disodium edetate, 20 parts by mass of sodium percarbonate, 15 parts by mass of sodium dodecyl alcohol polyoxyethylene ether sulfate, 600 parts by mass of deionized water In the mixed solution formed by mixing, ultrasonic vibration treatment was performed for 30 minutes. The temperature of the mixed solution was 70° C., then moved into 50° C. hot water for ultrasonic oscillation treatment for 60 minutes, and rinsed with water after taking it out.

[0040] (2) Place the inner surface of the metal pot body in a mixed solution mixed with 200 parts by mass of nickel sulfate, 60 parts by mass of sodium citrate, 50 parts by mass of ammonium chlori...

Embodiment 2

[0044] (1) The metal pot body is placed in 50 mass parts sodium silicate, 30 mass parts potassium hydroxide, 20-50 mass parts potassium carbonate, 15 mass parts citrate fatty acid glyceride, 5 mass parts ethylenediamine polyoxyethylene Polyoxypropylene block polyether, 20 parts by mass of sodium sulfate, 10 parts by mass of disodium edetate, 5 parts by mass of sodium percarbonate, 20 parts by mass of sodium lauryl alcohol polyoxyethylene ether sulfate, 800 parts by mass of In the mixed solution formed by mixing ionic water, ultrasonic vibration treatment was performed for 90 minutes. The temperature of the mixed solution was 50°C, and then moved into 80°C hot water for ultrasonic oscillation treatment for 30 minutes. After taking it out, rinse it with water.

[0045] (2) Place the inner surface of the metal pot body in a mixed solution mixed with 300 parts by mass of nickel sulfate, 45 parts by mass of sodium citrate, 90 parts by mass of ammonium chloride, 60 parts by mass of s...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention provides a high-temperature-resistant abrasion-resistant non-stick pan coating, a preparation method and a non-stick pan with the same. Nickel plating is conducted on the surface of a metal pan base body through the electrochemical method. Under the action of a magnetic field, a formed surface nickel layer is uniform and flat, and accordingly it is guaranteed that the subsequent coating is flat and uniform. Secondly, an annular structure in a poly(aryl ether nitrile ketone) molecular main chain makes the coating have good high temperature resistance, a molecular structure contains strong-polarity groups, namely nitrile groups, and the nitrile groups generate strong action force on the surface of a metal base material. Thirdly, under the action of irradiation, a silane coupling agent KH792 and poly(aryl ether nitrile ketone) have grafting reaction, and heat resistance is further improved, so that organic solvent molecules cannot permeate into the metal base material, stability is improved, the organic solvent molecules and the surface of the metal base material are connected in a strong chemical bond mode, and adhesion of the coating is greatly improved. Accordingly, the high-temperature-resistant anti-wear non-stick pan coating prepared through the method does not contain fluorine and is resistant to high temperature, abrasion and scratching.

Description

technical field [0001] The invention relates to the technical field of non-stick pans, in particular to a high-temperature-resistant and wear-resistant non-stick pan coating, a preparation method and a non-stick pan. Background technique [0002] Metal pots such as cast iron, stainless steel, aluminum, and aluminum alloy have been the most commonly used food cooking tools for a long time. There are problems such as sticking and burning of food, which not only damage the appearance of food, but also easily cause food to burn. Harmful ingredients such as benzopyrene and acrylamide are harmful to human health. In addition, the food residue adhering to the surface of the pot also brings difficulty to the cleaning of the pot. Non-stick pans have brought great convenience to people's lives because of their advantages such as easy cleaning, non-stick pans for frying / fried food, and less oily smoke, so they have been favored by people since their inception. [0003] At present, th...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C09D171/00C09D7/61C09D7/63C25D3/12C25D5/00C25D5/34C23G1/14A47J27/00A47J36/02A47J36/04
CPCA47J27/00A47J36/025A47J36/04C08K3/34C09D7/61C09D171/00C23G1/14C25D3/12C25D5/006C25D5/34
Inventor 肖彬彭彩佑王高林
Owner NINGBO GRAMMY KITCHENWARE
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products