Composite new building anticorrosive material and preparation method thereof

An anti-corrosion material and construction technology, applied in anti-corrosion coatings, anti-fouling/underwater coatings, epoxy resin coatings, etc., can solve the problems of heat resistance, poor weather resistance, inconvenient preparation and construction, short service life, etc. The effect of excellent corrosion performance, improved mechanical properties and convenient construction

Inactive Publication Date: 2019-01-15
MINGGUANG FEIZHOU NEW MATERIAL
View PDF2 Cites 2 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, the existing anti-corrosion coatings have single functions, poor heat resistance and weather resistance, short service life, and are not convenient for preparation and construction.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Composite new building anticorrosive material and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0043] A composite novel building anticorrosion material, which is made of the following raw materials in parts by mass:

[0044] 2-3 parts of nano titanium dioxide, 0.8-1 part of inert metal, 1-3 parts of plasticizer, 30-40 parts of organic resin, 40-50 parts of epoxy resin, 5-10 parts of filler, 1-3 parts of defoamer , 0.6-0.8 parts of film-forming aids, 1-3 parts of dispersants, 2-4 parts of preservatives and 15-20 parts of water.

[0045] 2. Wherein, described nano-titanium dioxide is anatase type nano-titanium dioxide.

[0046] The inert metal includes at least one of platinum, iridium and silver.

[0047] The plasticizer is cellulose, and the cellulose is modified fiber ester.

[0048] The fillers include talc, heavy calcium and clay.

[0049] The preparation of the composite novel building anticorrosion material comprises the following steps:

[0050] According to the above-mentioned mass parts, take each raw material required by the composite new building anticorro...

Embodiment 2

[0055] A composite novel building anticorrosion material, which is made of the following raw materials in parts by mass:

[0056] 3 parts of nano titanium dioxide, 0.9 parts of inert metal, 2 parts of plasticizer, 35 parts of organic resin, 45 parts of epoxy resin, 15 parts of filler, 2 parts of defoamer, 0.7 part of film-forming aid, 2 parts of dispersant, anti-corrosion 3 parts of agent and 15 parts of water.

[0057] Wherein, the nano titanium dioxide is anatase nano titanium dioxide.

[0058] The inert metal includes at least one of platinum, iridium and silver.

[0059] The plasticizer is cellulose, and the cellulose is modified fiber ester.

[0060] The fillers include talc, heavy calcium and clay.

[0061] The preparation of the composite novel building anticorrosion material comprises the following steps:

[0062] S1: Grinding: Pour the inert metal, plasticizer, organic resin, epoxy resin, filler and water into the grinder for grinding, so that the fineness of each...

Embodiment 3

[0066] A composite novel building anticorrosion material, which is made of the following raw materials in parts by mass:

[0067] 4 parts of nano-titanium dioxide, 1 part of inert metal, 3 parts of plasticizer, 40 parts of organic resin, 50 parts of epoxy resin, 20 parts of filler, 3 parts of defoamer, 0.8 part of film-forming aid, 3 parts of dispersant, anti-corrosion 4 parts of agent and 20 parts of water.

[0068] Wherein, the vitamin composition includes the following raw material components: the nano-titanium dioxide is anatase-type nano-titanium dioxide.

[0069] The inert metal includes at least one of platinum, iridium and silver.

[0070] The plasticizer is cellulose, and the cellulose is modified fiber ester.

[0071] The fillers include talc, heavy calcium and clay.

[0072] The preparation of the composite novel building anticorrosion material comprises the following steps:

[0073] S1: Grinding: Pour the inert metal, plasticizer, organic resin, epoxy resin, fi...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a composite new building anticorrosive material and a preparation method thereof. The composite new building anticorrosive material is made of the following raw materials by mass parts: 2-4 parts of nano titanium dioxide, 0.8-1 part of an inert metal, 1 to 3 parts of a plasticizer, 30 to 40 parts of organic resin, 40 to 50 parts of epoxy resin, 10 to 20 parts of a filler, 1to 3 parts of an antifoaming agent, 0.6 to 0.8 part of a film forming aid, 1 to 3 parts of a dispersing agent, 2 to 4 portions of preservatives and 10 to 20 parts of water. The composite new buildinganticorrosive material can degrade nitrogen oxides in air, and also has the functions of sterilization, anti-virus and self-purification, by adding of the inert metal, the activity of the material isimproved, the toughness of the new material is greatly improved, the mechanical properties of the material are improved, the construction is convenient, the preparation method is simple, and the waterproof, mildewproof and anticorrosive properties are excellent.

Description

technical field [0001] The invention relates to the technical field of preparation of new building materials, in particular to a composite novel building anticorrosion material and a preparation method thereof. Background technique [0002] The acids, alkalis, salts and aggressive solvents used and produced in the industrial production process, the aggressive media contained in the atmosphere, groundwater, surface water, and soil will all corrode buildings. In addition, buildings are subject to biocorrosion. Principles of building anti-corrosion design: limit the scope of action of corrosive media; dilute and discharge corrosive media; take protective measures in terms of architectural layout, structural selection, node construction and material selection. Anti-corrosion coatings, generally divided into conventional anti-corrosion coatings and heavy-duty anti-corrosion coatings, are an indispensable coating in paint coatings. Conventional anti-corrosion coatings play an ...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C09D163/00C09D5/08C09D5/14C09D7/61C09D7/65
CPCC08K2003/0806C08K2003/2241C08K2003/265C08K2201/011C08L2205/03C09D5/08C09D5/14C09D7/61C09D7/65C09D163/00C08L83/08C08L1/08C08K3/00C08K3/22C08K3/08C08K3/34C08K3/26C08K3/346
Inventor 顾文宇
Owner MINGGUANG FEIZHOU NEW MATERIAL
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products