A method for recovering gold from gold smelting slag
A technology of smelting slag and recovering gold, which is applied in the field of gold recovery, can solve the problems of complex process and not gold recovery, and achieve the effect of simple process, promoting gold leaching and good stability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0040] In the present embodiment, according to parts by weight, the composition of the gold leaching agent is: 20 parts of carbonized sodium cyanurate, 20 parts of sodium oxide,
[0041] 40 parts of sodium thiosulfate, 0.5 part of polyferric sulfate, 1 part of ammonium chloride;
[0042] A method for recovering gold from gold smelting slag, comprising the following steps:
[0043] (1) Break 2 kg of gold smelting slag (gold grade 687.58 g / t) to below 2 mm;
[0044] (2) put it into a titanium reactor, and soak it in hydrochloric acid with a mass concentration of 31% for 48 hours;
[0045] (3) washing the leaching residue with water until the pH value of the filtrate is 7, filtering to obtain a filter cake;
[0046] (4) Add water to the filter cake, and add calcium oxide to adjust the pH value to 10.5, adjust the slurry, and obtain a slurry with a mass percentage of 40%;
[0047] (5) In terms of the mass of gold smelting slag, add the gold leaching agent of 2000g / t in the slur...
Embodiment 2
[0049] In this example, according to parts by weight, the gold leaching agent includes the following components: 40 parts of carbonized sodium cyanurate, 10 parts of sodium oxide,
[0050] 20 parts of sodium thiosulfate, 5 parts of polyferric sulfate, 15 parts of ammonium chloride;
[0051] A method for recovering gold from gold smelting slag, comprising the following steps:
[0052] (1) Break 2 kg of gold smelting slag (gold grade 687.58 g / t) to <2 mm;
[0053] (2) Put it into a titanium reactor and soak it in hydrochloric acid with a mass concentration of 33% for 72 hours;
[0054] (3) washing the leaching residue with water until the pH value of the filtrate is 7, filtering to obtain a filter cake;
[0055] (4) Add water in the filter cake, and add calcium oxide to adjust the pH value to 11, adjust the slurry, and obtain a slurry with a mass percentage of 45%;
[0056] (5) In terms of the mass of gold smelting slag, add the gold leaching agent of 3000g / t in the slurry, t...
Embodiment 3
[0058] In this example, according to parts by weight, the composition of the gold leaching agent is: 20 parts of carbonized sodium cyanurate, 20 parts of sodium oxide, 40 parts of sodium thiosulfate, 0.5 parts of polyferric sulfate, and 1 part of ammonium chloride;
[0059]A method for recovering gold from gold smelting slag, comprising the following steps:
[0060] (1) Break 2 kg of gold smelting slag (gold grade 687.58 g / t) to <2 mm;
[0061] (2) put it into a titanium reactor, and soak it in hydrochloric acid with a mass concentration of 31% for 48 hours;
[0062] (3) washing the leaching residue with water until the pH value of the filtrate is 7, filtering to obtain a filter cake;
[0063] (4) Add water to the filter cake, and add calcium oxide to adjust the pH value to 10.5, adjust the slurry, and obtain a slurry with a mass percentage of 40%;
[0064] (5) Divide calcium peroxide with a total amount of 250g / t (in terms of the mass of gold smelting slag) into 5 parts, ea...