A mixed rare earth-transition element doped up-conversion laser crystal and its preparation method
A transition element, mixed rare earth technology, applied in lasers, crystal growth, laser parts and other directions, can solve problems such as low efficiency, achieve wide emission spectrum, high thermal conductivity, and achieve the effect of laser output
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] Mixed rare earth-transition element doped up-conversion laser crystal, the up-conversion laser crystal is graphene quantum dots: Yb 3+ / Er 3+ :NaYF 4 / ZrF 4 ; The up-conversion laser crystal includes a mixed crystal of yttrium tetrafluoride sodium and zirconium tetrafluoride in a molar ratio of 100:1 as a matrix, doped with 2.8% (mole percentage, the same below) of Yb 3+ As a sensitizer, doped with 1.2% Er 3+ As an activator, 0.018% graphene quantum dots were doped.
[0029] Its preparation method comprises the following steps:
[0030] (1) monolayer graphene oxide is added in polyvinyl alcohol aqueous solution to make the graphene oxide dispersion that concentration is 6mg / mL, add the polymethylpyrrolidone of ytterbium oxide, erbium oxide and 4 times monolayer graphene oxide quality, After the dispersion is uniform, transfer to the crucible, place the crucible in a muffle furnace for calcination, wash the solid mixture in the crucible with hot water at 75°C, and d...
Embodiment 2
[0036] Mixed rare earth-transition element doped up-conversion laser crystal, the up-conversion laser crystal is graphene quantum dots: Yb 3+ / Er 3+ :NaYF 4 / ZrF 4 ; The up-conversion laser crystal includes a mixed crystal of sodium tetrafluoroyttrium and zirconium tetrafluoride with a molar ratio of 100:0.5 as a host, doped with 1% Yb 3+ As a sensitizer, doped with 1.5% Er3+ As an activator, 0.005% graphene quantum dots were doped.
[0037] Its preparation method comprises the following steps:
[0038] (1) Add single-layer graphene oxide to polyvinyl alcohol aqueous solution to obtain a graphene oxide dispersion with a concentration of 2 mg / mL to 10 mg / mL, add ytterbium oxide, erbium oxide and 3 to 5 times the mass of single-layer graphene oxide After the polymethylpyrrolidone is uniformly dispersed, it is transferred to a crucible, and the crucible is placed in a muffle furnace for calcination, and the solid mixture in the crucible is washed with hot water at 60-90°C, an...
Embodiment 3
[0044] Mixed rare earth-transition element doped up-conversion laser crystal, the up-conversion laser crystal is graphene quantum dots: Yb 3+ / Er 3+ :NaYF 4 / ZrF 4 ; The up-conversion laser crystal includes a mixed crystal of sodium tetrafluoroyttrium and zirconium tetrafluoride in a molar ratio of 100:5 as a matrix, doped with 5% Yb 3+ As a sensitizer, doped with 0.5% Er 3+ As an activator, 0.03% graphene quantum dots were doped.
[0045] Its preparation method is identical with embodiment 2.