Five-membered copolymer fluid loss agent and preparation method thereof
A technology of fluid loss reducer and copolymer, applied in chemical instruments and methods, drilling compositions, etc., to achieve the effects of good reproducibility, inhibition of hydration swelling, and enhanced adsorption
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0016] A kind of pentapolymer fluid loss reducer and preparation method thereof, it comprises the steps:
[0017] 1) Dissolve 0.041mol of acrylic acid, 0.032mol of 2-acrylamide-2-methylpropanesulfonic acid, and 0.025mol of methacryloyloxyethyltrimethylammonium chloride in 70mL of water, and then use the mass percentage concentration of 20% sodium hydroxide solution adjusts the pH value of the system, the pH value is 7, and the mixed solution G is obtained;
[0018] 2) In the mixed solution G, add 0.208 mol of acrylamide and 0.010 mol of acrylonitrile to obtain a mixed solution H, and the mass percentage concentration of the mixed solution H is 30%;
[0019] 3) Heating the mixed solution H to 50° C., adding the initiator ammonium persulfate and sodium bisulfite successively, the molar ratio is 1:1, the amount of the initiator is 1.6% of the total mass of the monomer, and reacting for 10 minutes under constant stirring, Observe the viscosity, and let it stand in a constant temp...
Embodiment 2
[0023] A kind of pentapolymer fluid loss reducer and preparation method thereof, it comprises the steps:
[0024] 1) Dissolve 0.047mol of acrylic acid, 0.032mol of 2-acrylamide-2-methylpropanesulfonic acid, and 0.025mol of dimethyl diallyl ammonium chloride in 70mL of water, and then use 20% mass percent Sodium hydroxide solution adjusts the pH value of the system, and the pH value is 7 to obtain mixed solution G;
[0025] 2) In the mixed solution G, add 0.199 mol of acrylamide and 0.012 mol of acrylocyanide to obtain a mixed solution H, and the mass percentage concentration of the mixed solution H is 30%;
[0026] 3) Heating the mixed solution H to 50° C., adding the initiator ammonium persulfate and sodium bisulfite successively, the molar ratio is 1:1, the amount of the initiator is 1.6% of the total mass of the monomer, and reacting for 10 minutes under constant stirring, Observe the viscosity, and let it stand in a constant temperature water bath for 3 hours;
[0027] 4...
Embodiment 3
[0030] A kind of pentapolymer fluid loss reducer and preparation method thereof, it comprises the steps:
[0031] 1) Dissolve 0.043mol of acrylic acid, 0.033mol of 2-acrylamide-2-methylpropanesulfonic acid, and 0.026mol of methacryloxyethyltrimethylammonium chloride in 70mL of water, and then use the mass percentage concentration of 20% sodium hydroxide solution adjusted the pH value of the system, the pH value was 8, and mixed solution G was obtained;
[0032] 2) In the mixed solution G, add 0.217 mol of acrylamide and 0.010 mol of acrylonitrile to obtain a mixed solution H, and the mass percentage concentration of the mixed solution H is 30%;
[0033] 3) Heating the mixed solution H to 45° C., adding the initiator ammonium persulfate and sodium bisulfite successively, the molar ratio is 1:1, the amount of the initiator is 1.0% of the total mass of the monomer, and reacting for 10 minutes under constant stirring, Observe the viscosity, and let it stand in a constant temperat...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology