Preparation and preparation process for purifying storage environment and regulating environmental humidity
A technology of environmental humidity and preparation process, which is applied in the direction of air humidification system, other chemical processes, lighting and heating equipment, etc., can solve the problems of great influence of temperature, uncontrollable, high cost, etc., and achieve fast moisture absorption, large moisture absorption, Ease of use
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0081] Step 1: Prepare Purifying and Humidifying Agent
[0082] 1. Choose diatomite (SiO2) produced in Shandong 2 >80%, surface area ≥12m 2 / g, fineness 80 orders); choose the stilbinite powder (fineness 60 orders) that Fu Xin produces;
[0083] 2. Mix diatomaceous earth, zeolite, alkali and salt according to 45:50:3.5:1.5;
[0084] 3. Sinter the mixture in a 400-degree muffle furnace for 25 minutes;
[0085] 4. Break the sintered block into irregular granules of 1 to 2 cm;
[0086] 5. Mix the sintered material with the activated carbon of plant fruit core at 8:2;
[0087] 6. Packed with non-woven fabric, specification 100 grams, bag equipment.
[0088] Step 2: Strong Moisture Absorbent
[0089] 1. Choose edible starch (corn, potato or sweet potato), calcium chloride dihydrate (granular), Hebei Kuancheng perlite;
[0090] 2. The ratio of calcium chloride, starch and perlite is 50:40:10;
[0091] 3. Pack the mixture into a 200-gram bag with non-woven fabric for subseque...
Embodiment 2
[0096] Step 1: Prepare Purifying and Humidifying Agent
[0097] 1. Choose diatomite (SiO2) produced in Zhejiang 2 >85%, surface area ≥16m 2 / g, fineness 100 orders); choose the sodium zeolite powder (fineness 100 orders) that Chifeng produces;
[0098] 2. Mix diatomaceous earth, zeolite, alkali and salt according to 50:45:1.5:3.5;
[0099] 3. Sinter the mixture in a muffle furnace at 1200 degrees for 30 minutes;
[0100] 4. Break the sintered block into irregular granules of 3 to 4 cm;
[0101] 5. Mix the sintered material with coal activated carbon at a ratio of 6:4;
[0102] 6. Packed with non-woven fabric, specification 500 grams, bag equipment.
[0103] Step two:
[0104] 1. Choose calcium chloride (granular), pullulan, and perlite produced in Ningbo, Zhejiang;
[0105] 2. Calcium chloride:starch:perlite in a ratio of 65:30:5;
[0106] 3. Put the mixture in a bag made of polyethylene film, and pack it in a 100-gram bag;
[0107] 4. Take 10 sachets as a batch, and ...
Embodiment 3
[0111] step one:
[0112] 1. Choose the one produced in Linjiang, Jilin (SiO 2 >80%), diatomite (SiO 2 >91%, surface area ≥18m 2 / g, fineness 120 orders), choose the calcium zeolite powder (fineness 80 orders) that Shanxi Datong produces;
[0113] 2. Mix diatomaceous earth, zeolite, alkali and salt according to 55:40:3.5:1.5;
[0114] 3. Sinter the mixture in a 1000-degree muffle furnace for 35 minutes;
[0115] 4. Break the sintered block into irregular granular form ranging from 2 to 3 cm;
[0116] 5. Mix the sintered material with bamboo activated carbon at a ratio of 9:1;
[0117] 6. Packed with non-woven fabric, specification 500 grams, bag equipment.
[0118] Step two:
[0119] 1. Select pullulan, anhydrous calcium chloride (granular), and perlite produced in Lingqiu, Shanxi;
[0120] 2. The ratio of calcium chloride, starch and perlite is 60:30:10;
[0121] 3. Pack the mixture quickly with polyolefin or polyester non-woven fabric, 500g / bag;
[0122] 4. A batch...
PUM
Property | Measurement | Unit |
---|---|---|
Fineness | aaaaa | aaaaa |
Surface area | aaaaa | aaaaa |
Fineness | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com