A kind of preparation method using diethylenetriamine as raw material coal-based chelating adsorbent
A technology of diethylenetriamine and chelating adsorbent, which is applied in chemical instruments and methods, adsorption water/sewage treatment, and other chemical processes, can solve the problems of high manufacturing cost and complexity, and achieve good adsorption performance and good adsorption Performance, the effect of easy solid-liquid separation
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0028] The present embodiment takes 10g of coal dust as an example, and the method for preparing a coal-based chelating adsorbent with diethylenetriamine as a raw material is realized by the following steps:
[0029] (1) Weigh 10 g of raw coal powder with a particle size of 0.075 to 0.113 mm, add it to 100 mL of distilled water, mix well, weigh 0.3 g γ-aminopropyltriethoxysilane and add it to the coal powder solution to make the raw coal powder The mass ratio of γ-aminopropyltriethoxysilane to γ-aminopropyltriethoxysilane is 1:0.03, and the coupling reaction is stirred at 70°C for 3 hours to obtain coupled modified coal powder.
[0030] (2) Measure 5.15g of diethylenetriamine, add it to the coupling modified coal powder, make the mass ratio of raw coal powder and diethylenetriamine 1:0.515, and react at 60°C for 2 hours to obtain amine pulverized coal;
[0031] (3) Add 6g sodium hydroxide and 7.6g carbon disulfide to the aminated coal powder of step (2), that is, the mass rat...
Embodiment 2
[0033] The present embodiment takes 10g of coal dust as an example, and the method for preparing a coal-based chelating adsorbent with diethylenetriamine as a raw material is realized by the following steps:
[0034] (1) Same as step (1) of Example 1.
[0035] (2) Measure 4g of diethylenetriamine, add it to the coupling modified coal powder, make the mass ratio of raw coal powder and diethylenetriamine 1:0.4, and react at 50°C for 3 hours to obtain amination pulverized coal;
[0036] (3) Add 5g sodium hydroxide and 6.3g carbon disulfide to the aminated coal powder of step (2), make the mass ratio of raw coal powder, sodium hydroxide and carbon disulfide be 1:0.5:0.63, react for 1 hour at 35°C, A coal-based chelating adsorbent is obtained.
Embodiment 3
[0038] The present embodiment takes 10g of coal dust as an example, and the method for preparing a coal-based chelating adsorbent with diethylenetriamine as a raw material is realized by the following steps:
[0039] (1) Same as step (1) of Example 1.
[0040] (2) Measure 6g of diethylenetriamine, add it to the coupling modified coal powder, make the mass ratio of raw coal powder and diethylenetriamine 1:0.6, and react at 65°C for 2 hours to obtain amination pulverized coal;
[0041] (3) Add 7g sodium hydroxide and 8.32g carbon disulfide to the aminated coal powder of step (2), make the mass ratio of raw coal powder, sodium hydroxide and carbon disulfide be 1:0.7:0.832, react for 4 hours at 35°C, A coal-based chelating adsorbent is obtained.