Colored glazed quartz colorful sand and preparation method thereof
A quartz sand and fossil technology is applied in the field of colored and glazed quartz sand and its preparation, which can solve the problems of unstable hue, monotonous color, restricting the development of real stone paint, etc.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0036] A colored glazed quartz colored sand (white sand), which is made by mixing the following raw materials in parts by weight:
[0037] Quartz sand (10-20 mesh) 1000 parts,
[0038] Inorganic pigment (90% muscovite + 10% titanium dioxide) 10 parts,
[0039] Medium and low temperature glaze (calcium oxide + sodium carbonate + feldspar mixed in a weight ratio of 1:1:1) 10 parts,
[0040] High temperature resistant adhesive (sodium silicate) 5 parts,
[0041] Nano barium sulfate powder (particle size 50-100nm) 5 parts,
[0042] Nano silver powder (particle size 50-100nm) 1 part,
[0043] Dispersant (sodium polyacrylate) 2 parts,
[0044] 20 parts of water.
[0045] Muscovite is used after pre-treatment, and the pre-treatment includes the following steps:
[0046] (1) Calcination: calcining muscovite fragments at 650°C for 75 minutes to obtain cooked mica material, and then passing through a 15-20 mesh sieve;
[0047] (2) Impregnation: Immerse the sieved cooked mica mate...
Embodiment 2
[0051] A colored glazed quartz colored sand (black sand), which is made by mixing the following raw materials in parts by weight:
[0052] Quartz sand (100-120 mesh) 1000 parts,
[0053] Inorganic pigments (biotite 70% + cobalt black 30%) 20 parts,
[0054] Medium and low temperature glaze (calcium oxide + feldspar + zinc oxide + borax + kaolin mixed according to the weight ratio of 1:1:1:1:1) 20 parts,
[0055] High temperature resistant adhesive (sodium silicate + silica sol mixed in a weight ratio of 1:1) 10 parts,
[0056] Nano barium sulfate powder (particle size 50-100nm) 8 parts,
[0057] Nano silver powder (particle size 50-100nm) 3 parts,
[0058] Dispersant (sodium tripolyphosphate) 5 parts,
[0059] 40 parts of water.
[0060] Biotite is used after pre-treatment. The pre-treatment includes the following steps:
[0061] (1) Calcination: Calcinate biotite fragments at 900°C for 45 minutes to obtain cooked mica material, and then pass through a 15-20 mesh sieve;
...
Embodiment 3
[0066] A colored glazed quartz colored sand (yellow sand), which is made by mixing the following raw materials in parts by weight:
[0067] Quartz sand (40-60 mesh) 1000 parts,
[0068] Inorganic pigments (phlogopite 80% + iron oxide yellow 19% + titanium dioxide 1%) 15 parts,
[0069] Medium and low temperature glaze (calcium oxide + sodium carbonate + feldspar + kaolin mixed according to the weight ratio of 1:1:1:1) 15 parts,
[0070] High temperature resistant adhesive (aluminum dihydrogen phosphate) 8 parts,
[0071] Nano barium sulfate powder (particle size 50-100nm) 7 parts,
[0072] Nano silver powder (particle size 50-100nm) 2 parts,
[0073] Dispersant (sodium polyacrylate) 4 parts,
[0074] 30 parts of water.
[0075] Phlogopite is used after pretreatment, and the pretreatment includes the following steps:
[0076] (1) Calcination: Calcinate phlogopite fragments at 800°C for 60 minutes to obtain cooked mica material, and then pass through a 15-20 mesh sieve;
...
PUM
Property | Measurement | Unit |
---|---|---|
particle diameter | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com