A method for imitation silk reactive printing
A technology of reactive printing and imitation silk, which is applied in the field of textile printing and dyeing, can solve the problems of low product quality, increased equipment loss, and use restrictions, etc., and achieve the effect of soft and smooth hand feeling, reduced loss, and rich layers
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] A method for imitation silk active printing, the steps are as follows:
[0038] (1) Fabric pretreatment: Put the imitation silk cloth into the pretreatment agent for pretreatment
[0039] Pretreatment agent is made up of the raw material of following parts by weight:
[0040] Trehalose 1 part
[0041] Collagen 1.5 parts
[0042] 50 parts of water
[0043] (2) Sizing: The pretreated imitation silk cloth is sizing on a sizing machine, and the sizing is composed of the following raw materials in parts by weight:
[0044] Phosphate grafted starch 0.5 part
[0045] 4 parts sodium alginate
[0046] Nano titanium dioxide 1 part
[0047] Baking soda 3 parts
[0048] Yuan Mingfen 2 parts
[0049] 4 parts urea
[0050] Triethylene glycol 1 part
[0051] 40 parts of water
[0052] Mix the above components and put them into a beater, beat until the slurry is uniform, and then let it stand for 2 hours;
[0053] (3) Heating and shaping: Two hot blankets are pressed and he...
Embodiment 2
[0058] A method for imitation silk active printing, the steps are as follows:
[0059] (1) Fabric pretreatment: Put the imitation silk cloth into the pretreatment agent for pretreatment
[0060] Pretreatment agent is made up of the raw material of following parts by weight:
[0061] Trehalose 2 parts
[0062] Collagen 1 part
[0063] 60 parts of water
[0064] (2) Sizing: The pretreated imitation silk cloth is sizing on a sizing machine, and the sizing is composed of the following raw materials in parts by weight:
[0065] Phosphate grafted starch 1.5 parts
[0066] 3 parts sodium alginate
[0067] Nano titanium dioxide 1.5 parts
[0068] Baking soda 2 parts
[0069] Yuan Mingfen 3 parts
[0070] 3 parts urea
[0071] Triethylene glycol 1 part
[0072] 50 parts of water;
[0073] Mix the above components and put them into a beater, beat until the slurry is uniform, and then let it stand for 2 hours;
[0074] (3) Heating and shaping: Two hot blankets are pressed and...
Embodiment 3
[0079] A method for imitation silk active printing, the steps are as follows:
[0080] (1) Fabric pretreatment: Put the imitation silk cloth into the pretreatment agent for pretreatment
[0081] Pretreatment agent is made up of the raw material of following parts by weight:
[0082] Trehalose 1 part
[0083] Collagen 1.4 parts
[0084] 55 parts of water
[0085] (2) Sizing: The pretreated imitation silk cloth is sizing on a sizing machine, and the sizing is composed of the following raw materials in parts by weight:
[0086] Phosphate grafted starch 0.7 part
[0087] 4 parts sodium alginate
[0088] Nano titanium dioxide 1.1 parts
[0089] Baking soda 3 parts
[0090] Yuan Mingfen 2 parts
[0091] 4 parts urea
[0092] Triethylene glycol 1 part
[0093] 42 parts of water
[0094] Mix the above components and put them into a beater, beat until the slurry is uniform, and then let it stand for 2 hours;
[0095] (3) Heating and shaping: Two hot blankets are pressed and h...