A cast-in-place color continuous blind road and its manufacturing method
A blind road and color technology, which is applied in the field of cast-in-place color continuous blind road and its production, can solve problems such as uneven blind road, safety accidents, etc., achieve short construction time, strong anti-pollution ability, reduce road construction costs and material loss  Effect
- Summary
- Abstract
- Description
- Claims
- Application Information
 AI Technical Summary 
Problems solved by technology
Method used
Examples
Embodiment 1
[0021] A kind of cast-in-place color continuous blind road provided by the present invention, component A and component B, the mass ratio of component A and component B is 1: 4 ~ 6;
[0022] Group A is calculated in parts by weight, and its raw material composition includes the following components:
[0023] 70 parts of water-based epoxy acrylic hybrid emulsion, 5 parts of propylene glycol phenyl ether, 10 parts of water-based fatty amine crosslinking agent and 5 parts of deionized water;
[0024] Component B, in terms of parts by weight, its raw material composition includes the following components:
[0025] 35 parts of Portland cement, 55 parts of quartz sand, 3 parts of calcium carbonate, 2 parts of iron yellow pigment, 0.5 part of anti-crack fiber, 0.3 part of methyl cellulose, 0.1 part of early strength agent and 0.05 part of water reducing agent.
[0026] Among them, Portland cement is 425# Portland cement.
[0027] Waterborne epoxy acrylic hybrid emulsion: It has exc...
Embodiment 2
[0048] This embodiment is basically the same as Embodiment 1, and its performance is the same as that of Embodiment 1. The difference is that in this embodiment, a cast-in-place color continuous blind walkway, component A is calculated in parts by weight, and its raw material composition includes the following components :
[0049] 80 parts of water-based epoxy acrylic hybrid emulsion, 8 parts of propylene glycol phenyl ether, 15 parts of water-based fatty amine crosslinking agent and 10 parts of deionized water;
[0050] Component B, in terms of parts by weight, its raw material composition includes the following components:
[0051] 40 parts of Portland cement, 60 parts of quartz sand, 5 parts of calcium carbonate, 5 parts of pigment iron yellow, 1 part of anti-crack fiber, 0.5 part of methyl cellulose, 0.3 part of early strength agent and 0.1 part of water reducing agent.
Embodiment 3
[0053]This embodiment is basically the same as Embodiment 1, and its performance is the same as that of Embodiment 1. The difference is that in this embodiment, a cast-in-place color continuous blind walkway, component A is calculated in parts by weight, and its raw material composition includes the following components :
[0054] 75 parts of water-based epoxy acrylic hybrid emulsion, 7 parts of propylene glycol phenyl ether, 12 parts of water-based aliphatic amine crosslinking agent and 8 parts of deionized water;
[0055] Component B, in terms of parts by weight, its raw material composition includes the following components:
[0056] 38 parts of Portland cement, 58 parts of quartz sand, 4 parts of calcium carbonate, 3 parts of iron yellow pigment, 0.8 part of anti-crack fiber, 0.4 part of methyl cellulose, 0.2 part of early strength agent and 0.08 part of water reducing agent.
PUM
 Login to View More
 Login to View More Abstract
Description
Claims
Application Information
 Login to View More
 Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com