A technology of blood purification and montmorillonite, which is applied in chemical instruments and methods, blood circulation treatment, and other chemical processes, can solve problems such as poor adsorption selectivity, poor blood compatibility, and hemodynamic instability, and achieve good Blood compatibility, the effect of safe use
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0033] 1) Weigh 1Kg of the separated and purified calcium-based montmorillonite, add 9 liters of water, and stir evenly to make a suspension. Add 150g NaCl, stir evenly (about 20 minutes) and heat to about 60°C, ion exchange reaction for six hours, stirring from time to time. Then centrifuge to settle, pour off the supernatant, add 9 liters of water, stir evenly, continue to centrifuge, pour off the supernatant. Repeat 3 to 4 times, dehydrate again, dry at 80°C, grind to less than 300 mesh, and obtain sodium-based montmorillonite powder.
[0034] 2) Add 40 g of chitosan and 40 g of gelatin to 1 liter of distilled water, heat and stir in a water bath at 60° C. until completely dissolved.
[0035] 3) Weigh 300g of sodium-based montmorillonite powder, add it into the chitosan and gelatin solution, stir evenly, and keep the temperature in a water bath at 60° C. for 3 hours, stirring from time to time.
[0036] 4) Add a pre-prepared NaOH solution with a concentration of 1% into t...
Embodiment 2
[0039] 1) Add 40 g of chitosan and 40 g of agar in 1 liter of distilled water, heat and stir in a water bath at 50° C. until completely dissolved.
[0040] 2) Weigh 300 g of separated and purified sodium-based montmorillonite powder, add it to the chitosan and agar solution, stir evenly, and keep the temperature in a water bath at 50° C. for 3 hours, stirring from time to time.
[0041] 3) Add pre-prepared sodium tripolyphosphate solution with a concentration of 1% into the container, and spray the suspension of sodium montmorillonite, chitosan and agar into the container while stirring.
[0042] 4) After continuing to stir gently for 20 minutes, centrifuge or filter to separate, wash with water until neutral, steam sterilize, dry at 80°C, and pack.
Embodiment 3
[0044] 1) Add 40 g of chitosan and 40 g of agar in 1 liter of distilled water, heat and stir in a water bath at 50° C. until completely dissolved.
[0045] 2) Weigh 300 g of separated and purified sodium-based montmorillonite powder, add it into the chitosan and agarose solution, stir evenly, and keep the temperature in a water bath at 50° C. for 3 hours, stirring from time to time.
[0046] 3) Add a pre-prepared sodium sulfate solution with a concentration of 1.5% into the container, and spray the suspension of sodium montmorillonite, chitosan and agarose into the container while stirring.
[0047] 4) After continuing to stir gently for 30 minutes, centrifuge or filter to separate, wash with water until neutral, steam sterilize, dry at 80°C, and pack.