[0016] Take by weighing 5 kilograms of No. 64 high-melting point paraffin wax (Fushun Petroleum No. 1 Plant), 6 kilograms of No. 80 petroleum microcrystalline wax (Jingmen Petrochemical Company); 5 kilograms of petroleum resin p-100 (Shanghai Petroleum Resin Co., Ltd.); 6 kilograms of isopropylamine (Taiyuan Fakai Chemical Company of China Daily Chemical Institute); 4 kilograms of dodecylamine (Taiyuan Fakai Chemical Company of China Daily Chemical Institute); polyoxyethylene (20) sorbitan monostearate 3 kilograms (Fushun Konka Chemical Co., Ltd.); 1 kilogram of sodium benzoate (Tianjin Dongda Chemical Co., Ltd.); the balance is purified water;
[0017] Its preparation method is:
[0018] ①. Add 5 kg of No. 64 high melting point paraffin wax, 6 kg of No. 80 petroleum microcrystalline wax, 5 kg of petroleum resin p-1005, and 6 kg of diisopropylamine benzoate into a stainless steel container and slowly heat to 130 ° C. The reaction time is 30 minutes Made into oil phase materia...
Embodiment 2
[0023] Take by weighing 4 kilograms of No. 70 high-melting point paraffin wax (Dalian Petroleum Company), 8 kilograms of No. 85 petroleum microcrystalline wax (Nanyang Fine Chemical Factory), 5 kilograms of synthetic rosin J-115 (Guilin Songquanlin Chemical Industry Co., Ltd.), benzene 8 kilograms of diisopropylamine formate (China Daily Chemical Institute Taiyuan Fakai Chemical Company), 4 kilograms of octadecylamine (China Daily Chemical Institute Taiyuan Fakai Chemical Company), polyoxyethylene (20) sorbitan monostearate 2 kilograms of acid esters (Fushun Konka Chemical Co., Ltd.), 1 kilogram of borax (Tianjin Dongda Chemical Co., Ltd.), and the balance is distilled water.
[0024] Its preparation method is:
[0025] ①. Add 4 kg of No. 70 high melting point paraffin wax; 8 kg of No. 85 petroleum microcrystalline wax, 1155 kg of synthetic rosin J-115, and 8 kg of diisopropylamine benzoate into a stainless steel container and slowly heat to 125°C, and the reaction time is 35 ...
Embodiment 3
[0030] Take by weighing 5 kilograms of No. 68 high melting point paraffin wax (Dalian Petroleum Company), 12 kilograms of No. 85 oxidized microcrystalline wax (Fushun Petroleum Research Institute), 4 kilograms of synthetic rosin J-115 (Guilin Songquanlin Chemical Industry Co., Ltd.), petroleum 3 kilograms of resin p-90 (Shanghai Petroleum Resin Co., Ltd.), 7 kilograms of diisopropylamine benzoate (China Daily Chemical Institute Taiyuan Fakai Chemical Company), 5 kilograms of octadecylamine (China Daily Chemical Institute Taiyuan Fakai Chemical Company ), 4 kilograms of polyoxyethylene (20) sorbitan monostearate (Fushun Konka Chemical Co., Ltd.), 1.3 kilograms of sodium benzoate (Tianjin Dongda Chemical Co., Ltd.), and the balance is distilled water.
[0031] Its preparation method is:
[0032] ①. Add 5 kg of No. 68 high melting point paraffin wax, 12 kg of No. 85 oxidized microcrystalline wax, 4 kg of synthetic rosin J-115, 3 kg of petroleum resin P-90, and 7 kg of diisopropyl...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com