A dendritic polyamine-based polymer drilling fluid for mud rock drilling
A technology of drilling fluid and polymer, which is applied in the field of drilling fluid, can solve the problems that can not completely solve the problem of shrinkage and sticking of clay mudstone formation, can not meet the environmental protection requirements of drilling engineering, and the performance of drilling fluid is not easy to control, so as to avoid water absorption swelling and dispersion , Improve drilling efficiency and reduce reservoir damage
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0037] Example 1 Inhibition of Xuanhua Bentonite Slurry and Temperature Resistance Evaluation
[0038] Add 35% Xuanhua bentonite to the drilling fluid formula 1, put it into the aging tank and roll and age at different temperatures for 16 hours, and measure the rheology of the drilling fluid after cooling to room temperature. The data are shown in Table 1.
[0039] Drilling fluid formula 1: 10 parts by weight of dendritic polyamine-based polymer; 4 parts by weight of bentonite in drilling fluid; 2 parts by weight of soda ash; 2 parts by weight of polymer coating agent; 2 parts by weight of potassium polyacrylate; hydrolyzed polyacrylonitrile ammonium salt 15 parts by weight; 10 parts by weight of anti-mud bag lubricant; 1000 parts by weight of water.
[0040] Table 1 Inhibition of Xuanhua bentonite pulping and temperature resistance (the following is the mass fraction)
[0041] drilling fluid Experimental conditions PV YP Drilling fluid formula 1+35% Xuanhu...
Embodiment 2
[0045] Example 2 Shale Rolling Recovery Rate Determination Test
[0046] Refer to "Zhang Xiaohua, Luo Xingshu, et al., "Modern Mud Experimental Technology" to suppress the shale dispersion experiment (page 45).
[0047] Drilling fluid formula 1: 10 parts by weight of dendritic polyamine-based polymer; 4 parts by weight of bentonite in drilling fluid; 2 parts by weight of soda ash; 2 parts by weight of polymer coating agent; 2 parts by weight of potassium polyacrylate; hydrolyzed polyacrylonitrile ammonium salt 15 parts by weight; 10 parts by weight of anti-mud bag lubricant; 1000 parts by weight of water.
[0048] Organic amine strong inhibition anti-slump drilling fluid: organic amine inhibitor G319-FTJ 1.0%-2.0%, organic inhibitor 0.3%-0.5%, viscosifier 0.3%-0.5%, low viscosity polyanionic cellulose PAC-LV 0.3-0.5%, high viscosity polyanionic cellulose PAC-HV 0.3-0.6%, barite 0-3%, preservative 0.05-0.2%, defoamer 0.1-0.3%, and the balance is water. (Refer to the Chinese p...
Embodiment 3
[0059] Embodiment 3 biological toxicity evaluation
[0060] Detected by China Oceanic Administration Tianjin Marine Monitoring Center Station, the LC of the present invention 50 The value is 35000mg / L, which is a non-toxic product.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com