Colored cigarette paper and preparation method thereof
A cigarette paper and colored technology, which is applied in the field of colored cigarette paper and its preparation, can solve the adverse effects of smoke quality, cannot reduce cigarette paper burnt gas, irritation and other problems, achieve good smoke compatibility and avoid potential safety hazards
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0022] Take 30L of water, add 5kg of alanine and 10Kg of glucose, add 300g of dipotassium hydrogen phosphate as a catalyst and a pH regulator, heat and stir at 95°C for 10 hours to obtain a colored solution containing melanoidin.
[0023] Add 10 kg of fire-accelerating agent potassium citrate into the obtained coloring solution, stir and dissolve completely to obtain a mixed sizing solution.
[0024] Take 400kg wood pulp fiber, add 15m 3 Water, add 150kg of calcium carbonate to the slurry according to the normal production process, and mix thoroughly to obtain a mixed slurry. The mixed slurry is subjected to sheet-forming, dehydration and primary drying to obtain a primary dry paper web with a moisture content of about 10%. The initial drying temperature is 65°C and the end temperature is 105°C.
[0025] Surface sizing and secondary drying were carried out on the primary dried paper web to obtain brown cigarette paper. The starting temperature of secondary drying is 38°C, a...
Embodiment 2
[0027] Take 20L of water, add 6kg of proline and 10Kg of fructose, add 500g of sodium phosphate as a catalyst and a pH regulator, heat and stir at 105°C for 8 hours to obtain a colored solution containing melanoidin.
[0028] Add 15kg of combustion accelerant potassium malate into the obtained colored solution, stir and dissolve completely to obtain a mixed sizing solution.
[0029] Take 500kg wood pulp fiber, add 18m 3 water, add 180kg of diatomaceous earth to the slurry according to the normal production process, and mix thoroughly to obtain a mixed slurry. The mixed slurry is subjected to sheet-forming, dehydration and primary drying to obtain a primary dry paper web with a moisture content of about 10%. The initial drying temperature is 65°C and the end temperature is 105°C.
[0030] Surface sizing and secondary drying were carried out on the primary dried paper web to obtain brown cigarette paper. The starting temperature of secondary drying is 38°C, and the ending tem...
Embodiment 3
[0032] Take 20L of water, add 3kg of lysine, 2Kg of histidine and 20Kg of invert syrup, add 1000g of potassium citrate as a catalyst and a pH regulator, heat and stir at 120°C for 12 hours to obtain a colored solution containing melanoidin.
[0033] Add 10kg of potassium citrate and 5kg of sodium citrate as combustion accelerants into the obtained coloring solution, stir and dissolve to obtain a mixed sizing solution.
[0034] Get 300kg wood pulp fiber and 200kg hemp pulp fiber, add 18m 3 Water, add 180kg of calcium carbonate in the slurry according to the normal production process, and mix thoroughly to obtain the mixed slurry. The mixed slurry is subjected to sheet-forming, dehydration and primary drying to obtain a primary dry paper web with a moisture content of about 10%. The initial drying temperature is 65°C and the end temperature is 105°C.
[0035] Surface sizing and secondary drying were carried out on the primary dried paper web to obtain brown cigarette paper. T...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.