A kind of inorganic water-in-sand colorful coating and preparation method thereof
A technology of multi-color coatings and water packs, applied in the direction of multi-color effect coatings, anti-corrosion coatings, alkali metal silicate coatings, etc., can solve problems such as poor hardness and water resistance, easy cracking of film formation, whitening of color spots, etc., and achieve high Effects of hardness and water resistance, excellent hardness, and stable storage viscosity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] An inorganic sand-in-water multi-color coating is prepared by mixing a protective colloid solution, a granulated base paint and a continuous phase;
[0032] In parts by mass, the protective colloid solution includes 90 parts of deionized water, 0.1 part of anti-settling agent, and 1 part of protective rubber powder; the granulated base paint includes 25 parts of deionized water, 0.5 part of cellulose ether, 1 part of kaolin 0.1 part of titanium dioxide, 10 parts of inorganic resin, 1 part of protective rubber powder, 0.1 part of color paste, 30 parts of 80-120 mesh snow white (sand); the continuous phase includes 40 parts of inorganic resin and 30 parts of deionized water , 0.1 part of multifunctional additive, 0.5 part of thickener;
[0033] Wherein, the inorganic resin is made of silicon acrylic emulsion, epoxy silane, amino silane, sodium silicate and silica sol, and the preparation steps are:
[0034] Step a), adjust the pH of 5 parts of aminosilane to 7 with aqueo...
Embodiment 2
[0046] An inorganic sand-in-water multi-color coating is prepared by mixing a protective colloid solution, a granulated base paint and a continuous phase;
[0047] In parts by mass, the protective colloid solution includes 94 parts of deionized water, 0.5 parts of anti-settling agent, and 5.5 parts of protective rubber powder; the granulated base paint includes 31.2 parts of deionized water, 1 part of cellulose ether, 3 parts of kaolin parts, 0.6 parts of titanium dioxide, 20 parts of inorganic resin, 4 parts of protective rubber powder, 0.2 parts of color paste, 40 parts of 80-120 mesh snowflake white; the continuous phase includes 50 parts of inorganic resin, 48.9 parts of deionized water, multi-functional 0.3 parts of additives, 0.8 parts of thickeners;
[0048] Among them, the inorganic resin is made of silicon acrylic emulsion, epoxy silane, amino silane, sodium silicate and silica sol, and the preparation steps are:
[0049] Step a), adjust the pH of 5 parts of aminosil...
Embodiment 3
[0062] An inorganic sand-in-water multi-color coating is prepared by mixing a protective colloid solution, a granulated base paint and a continuous phase;
[0063] In parts by mass, the protective colloid solution includes 100 parts of deionized water, 1 part of anti-settling agent, and 10 parts of protective rubber powder; the granulated base paint includes 35 parts of deionized water, 1.5 parts of cellulose ether, 10 parts of kaolin 1 part, 1 part of titanium dioxide, 30 parts of inorganic resin, 5 parts of protective rubber powder, 0.5 part of color paste, 50 parts of 80-120 mesh snowflake white; the continuous phase includes 70 parts of inorganic resin, 50 parts of deionized water, multi-functional 1 part of additive, 1 part of thickener;
[0064] Wherein, the inorganic resin is made of silicon acrylic emulsion, epoxy silane, amino silane, sodium silicate and silica sol, and the preparation steps are:
[0065] Step a), adjust the pH of 10 parts of aminosilane to 7 with aq...