Preparation method and application of copper-arsenic flotation separation inhibitor for mixed copper ore
A technology of mixing copper ore and inhibitor, applied in flotation, solid separation and other directions, can solve the problems of large amount of arsenic-containing minerals inhibition, decreased copper recovery rate, oxidation failure, etc., to achieve selective inhibition effect and good selectivity. Adsorption, elimination of activation effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] The preparation method of copper arsenic flotation separation inhibitor of mixed copper ore of the present invention comprises the following steps:
[0019] (1) Prepare a sulfuric acid solution with a mass concentration of 15%. After the water area is heated to 30-35°C, add the prepared mixed starch according to a solid-to-liquid ratio of 1:5, and stir and react at a constant temperature for 1.5 hours to obtain a reaction solution. Wherein, the mixed starch is tapioca starch and potato starch, and the preparation ratio is 3:1.
[0020] (2) Add sulfuric acid to the reaction solution in step (1) to adjust the pH to 6.0-6.5, then add thiourea according to the mass of thiourea:starch = 1:3, further raise the temperature of the solution to 90°C and stir for 45 minutes , the solution is a colorless transparent liquid after the reaction is completed;
[0021] (3) Add sodium hydroxide to the liquid obtained in step (2) to adjust the pH to 8.0-8.5, stir for about 30 minutes, co...
Embodiment 2
[0023] The preparation method of copper arsenic flotation separation inhibitor of mixed copper ore of the present invention comprises the following steps:
[0024] (1) Prepare a sulfuric acid solution with a mass concentration of 10%. After the water area is heated to 35-40°C, add the prepared mixed starch according to a solid-to-liquid ratio of 1:6, and stir and react at a constant temperature for 1.5 hours to obtain a reaction solution. Wherein, the mixed starch is tapioca starch and potato starch, and the preparation ratio is 2:1.
[0025] (2) Add sulfuric acid to the reaction solution in step (1) to adjust the pH to 6.0-6.5, then add thiourea according to the mass of thiourea:starch = 1:3, further raise the temperature of the solution to 90°C and stir for 45 minutes , the solution is a colorless transparent liquid after the reaction is completed;
[0026] (3) Add sodium hydroxide to the liquid obtained in step (2) to adjust the pH to 8.0-8.5, stir for about 30 minutes, co...
Embodiment 3
[0028] The preparation method of copper arsenic flotation separation inhibitor of mixed copper ore of the present invention comprises the following steps:
[0029] (1) Prepare a sulfuric acid solution with a mass concentration of 20%, heat the water area to 35-40°C, add the prepared mixed starch according to the solid-to-liquid ratio of 1:4, stir and react at a constant temperature for 1.5 hours to obtain a reaction solution. Wherein, the mixed starch is tapioca starch and potato starch, and the preparation ratio is 1:1.
[0030] (2) Add sulfuric acid to the reaction solution in step (1) to adjust the pH to 6.5-7.0, then add thiourea according to the mass of thiourea:starch = 1:3, further raise the temperature of the solution to 90°C and stir for 45 minutes , the solution is a colorless transparent liquid after the reaction is completed;
[0031] (3) Add sodium hydroxide to the liquid obtained in step (2) to adjust the pH to 8.0-8.5, stir for about 45 minutes, concentrate and...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com