Method for preparing sheet material adhesive
A production method and adhesive technology, applied in the preparation of adhesives, animal glue or gelatin, adhesive types, etc., can solve the problems of polluting the environment and human body, harmfulness, and release of formaldehyde, etc., to increase the probability of crosslinking and increase hydrophobicity , low cost effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] The present invention is a method for manufacturing a sheet adhesive, which includes the following steps:
[0024] A. Add 80 parts by weight of corn gluten meal to 500 parts by weight of water, stir evenly to obtain a corn gluten solution;
[0025] B. The zein solution obtained in step A is subjected to ultrasonic treatment with a power of 100-120W for 60 minutes at a temperature of 45-55°C;
[0026] C. Add 0.5 parts by weight of sodium dodecylbenzene sulfonate to the solution obtained in step B, and stir for 1 hour;
[0027] D. Add 5 parts by weight of boric acid to the solution obtained in step C, and stir for 1 hour;
[0028] E. Add 25 parts by weight of acetamide, 5 parts by weight of talc, 5 parts by weight of hydroxypropyl starch ether, 5 parts by weight of gum arabic, 5 parts by weight of dextrin, 5 parts by weight to the solution obtained in step D To obtain potassium sorbate, 5 parts by weight of benzoic acid and 5 parts by weight of sodium sulfite, stir evenly.
Embodiment 2
[0030] The present invention is a method for manufacturing a sheet adhesive, which includes the following steps:
[0031] A. Add 90 parts by weight of soy protein powder to 500 parts by weight of water and stir to obtain a soy protein solution;
[0032] B. The soybean protein solution obtained in step A is subjected to ultrasonic treatment with a power of 100-120W for 60 minutes, and the treatment temperature is 45-55°C;
[0033] C. Add 0.5 parts by weight of sodium dodecylbenzene sulfonate to the solution obtained in step B, and stir for 1 hour;
[0034] D. Add 5 parts by weight of boric acid to the solution obtained in step C, and stir for 1 hour;
[0035] E. To the solution obtained in step D, add 25 parts by weight of acetamide, 5 parts by weight of bentonite, 5 parts by weight of sodium alginate, 5 parts by weight of gelatin, 5 parts by weight of dextrin, 5 parts by weight of sorbic acid, 5 parts by weight of ethyl hydroxybenzoate and 5 parts by weight of sodium benzoate are obtai...
Embodiment 3
[0037] The present invention is a method for manufacturing a sheet adhesive, which includes the following steps:
[0038] A. Add 35 parts by weight of corn gluten meal and 50 parts by weight of porcine blood globulin powder to 500 parts by weight of water, and stir to obtain a protein solution;
[0039] B. The protein solution obtained in step A is subjected to ultrasonic treatment with a power of 100-120W for 60 minutes at a temperature of 45-55°C;
[0040] C. Add 0.5 parts by weight of sodium dodecylbenzene sulfonate to the solution obtained in step B, and stir for 1 hour;
[0041] D. Add 5 parts by weight of boric acid to the solution obtained in step C, and stir for 1 hour;
[0042] E. Add 25 parts by weight of acetamide, 5 parts by weight of bentonite, 5 parts by weight of sodium alginate, 5 parts by weight of gelatin, 5 parts by weight of dextrin, 5 parts by weight of sorbic acid, to the solution obtained in step D, 5 parts by weight of ethyl hydroxybenzoate and 5 parts by weight...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com