A beneficiation method and high-calcium-magnesium technology, applied in flotation, solid separation and other directions, can solve the problems of difficult separation and enrichment of tungsten-molybdenum fluorite, high content of calcium-magnesium gangue and mud-containing gangue, and low recovery rate. Achieve the effect of improving resource utilization rate, improving recovery rate and reducing medium mineral rate
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0064] Feed 1 is molybdenum sulfide flotation tailings from a tungsten-molybdenum-fluorite polymetallic mine in Henan, with Mo grade of 0.8%, WO 3 Grade 0.12%, CaF 2 The grade is 10.23% and the tailings fineness is -0.074mm containing 80%. The main useful minerals of molybdenum sulfide flotation tailings are molybdenum-tungsten calcium ore, scheelite, and fluorite; the intercalation particle size of useful minerals is mainly microfine, -0.045 accounts for 64%; calcite and dolomite are as high as 28%, and serpentine Contains 9%, montmorillonite contains 3%.
[0065] The test process is as figure 1 .
[0066] (1) Floating sulfur tailings desliming: use molybdenum sulfide flotation tailings as raw material, and use hydrocyclone to remove 6% of the mud.
[0067] (2) Classification, separation and separation: add 1500 g / t of sodium carbonate (that is, add 1500 grams of molybdenum sulfide flotation tailings dry ore in step 1 per ton, the same below) to the pulp after desliming d...
Embodiment 2
[0071] The difference from Example 1 is that the ore feeder 2 is molybdenum sulfide flotation tailings of a tungsten-molybdenum-fluorite polymetallic ore in Henan, the Mo grade is 0.76%, WO 3 Grade 0.10%, CaF 2 The grade is 9.8% and the tailings fineness is -0.074mm containing 80%. The main useful minerals of molybdenum sulfide flotation tailings are molybdenum-tungsten calcium ore, scheelite, and fluorite; the particle size of useful minerals is mainly fine, with -0.045 accounting for 47%; calcite and dolomite contain 27%, and serpentine contains 8%, montmorillonite contains 3%.
[0072] The difference in implementation is that after desliming, there are two types of floating tungsten, molybdenum and molybdenum fluorite, which are easy to separate and difficult to separate, and the floating coarse concentrate 2 after floating will not be reground before separation.
[0073] After mixed flotation, fluorite is inhibited from flotation molybdenum oxide and scheelite respective...