Two-component antibacterial mildew-proof sealant and preparation method thereof

An antibacterial, anti-mildew, beautifying agent technology, applied in the direction of adhesives, adhesive types, adhesive additives, etc., can solve the problems of beautifying agent functional limitations, lack of anti-virus function, easy residual virus, etc., to achieve optimal material addition Sequence, good anti-virus ability, stable effect

Pending Publication Date: 2021-06-11
杭州华圩新材料科技有限公司
View PDF2 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

However, the function of the current beauty joint agent is still relatively limited, and there is still a lack of anti-virus function of the beauty joint agent, so the beauty joint agent in some wet corners is very easy to breed viruses, and at the same time, the virus is easy to remain in the beauty joint after the infected person touches it agent surface

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Two-component antibacterial mildew-proof sealant and preparation method thereof
  • Two-component antibacterial mildew-proof sealant and preparation method thereof
  • Two-component antibacterial mildew-proof sealant and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0020] Embodiment 1: A two-component antibacterial and anti-mildew beautifying agent is prepared by the following method, and the contents of the following components are in weight percent. First prepare component A: the preparation of component A includes the following steps: S110: Add 72% bisphenol A epoxy resin to the reaction kettle, heat at 40-50°C, and stir for 15-20 minutes; S120: Add Bisphenol F type epoxy resin 8%, heat at 40-50°C, stir for 15-20 minutes; S130: Add 3% benzyl alcohol and 8% active diluent to the reaction kettle, heat at 40-50°C, stir for 15-20 minutes Minutes; S140: Add 4% of fumed silica, 0.6% of defoamer, 0.6% of thickener and 0.6% of functional additives to the reaction kettle, heat at 40-50°C, and stir for 15-20 minutes; S150: Add to the reaction kettle Add 0.1% of ultraviolet absorber, 0.3% of antioxidant, 0.5% of nano-immonite clay and 0.1% of graphene composite anti-virus powder into the kettle, heat at 40-50°C, and stir for 15-20 minutes; S160:...

Embodiment 2

[0022] Example 2: A two-component antibacterial and anti-mildew beautifying agent is prepared by the following method, and the contents of the following components are in weight percent. Including the preparation of component A and the preparation of component B, the preparation method is the same as in Example 1, but the weight percentages of the components are different. The weight percentages of the components in Example 2 are as follows: the weight percentages of the components in the preparation process of the A component are as follows : bisphenol A type epoxy resin 80%; bisphenol F type epoxy resin 3%; benzyl alcohol 8%; reactive diluent 3%; fumed silica 10%; defoamer 0.3%; thickener 0.3% 0.3% of functional additives; 0.2% of ultraviolet absorbers; 0.3% of antioxidants; 1.5% of graphene composite anti-virus powder; The weight percent of the components in the preparation process of the B component is as follows: 85% of modified amine curing agent; 18% of benzyl alcohol; ...

Embodiment 3

[0023]Embodiment 3: A two-component antibacterial and anti-mildew beautifying agent is prepared by the following method, and the contents of the following components are in weight percent. Including the preparation of component A and the preparation of component B, the preparation method is the same as in Example 1, and the weight percentages of the components are different. The weight percentages of the components in Example 3 are as follows: The A component includes the following components and weight percentages: double Phenol A type epoxy resin 76%; bisphenol F type epoxy resin 6%; benzyl alcohol 6%; reactive diluent 6%; fumed silica 7%; defoamer 0.5%; thickener 0.4%; function 0.5% additives; 0.16% UV absorber; 0.45% antioxidant; 1.1% graphene composite anti-virus powder; 0.8% nanometer clay. The B component includes the following components and weight percentages: 80% modified amine curing agent; 25% benzyl alcohol; 0.5% defoamer; 7% fumed white carbon black; 0.4% functio...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention relates to a two-component antibacterial mildew-proof sealant and a preparation method thereof. The sealant comprises a component A and a component B. The component A comprises the following components by weight: 72%-80% of bisphenol A epoxy resin, 3%-8% of bisphenol F epoxy resin, 4%-10% of fumed silica, 0.3%-0.6% of a defoaming agent, 0.3%-0.6% of a thickening agent, 0.3%-0.6% of a functional auxiliary agent, 0.1%-0.2% of an ultraviolet light absorber, 3%-8% of benzyl alcohol, 3%-8% of a reactive diluent, 0.3%-0.6% of an antioxidant, 0.1%-1.5% of graphene composite antiviral powder, and 0.5%-1% of nano illite-montmorillonite clay. The component B comprises the following components in percentage by weight: 70%-85% of a modified amine curing agent, 18%-30% of benzyl alcohol, 0.3%-0.6% of a defoaming agent, 4%-10% of fumed silica, 0.3%-0.6% of a functional auxiliary agent, 1%-2% of a flow stopping agent, 0.1%-1.5% of graphene composite antiviral powder, and 0.5%-1% of nano illite-montmorillonite clay. According to the two-component antibacterial mildew-proof sealant and the preparation method thereof, the graphene composite antiviral powder is added, so that the constructed product has good anti-virus capability; and in addition, a certain amount of illite-montmorillonite clay is added, so that the composite antiviral powderhas antibacterial, mildew-proof and formaldehyde-absorbing functions.

Description

technical field [0001] The invention belongs to the technical field of adhesives, and in particular relates to a two-component antibacterial and anti-mold beautifying agent, and at the same time, the invention also relates to a preparation method of the beautifying agent. Background technique [0002] During the house decoration process, many owners will choose to use tiles to pave the floor and walls, and the decoration effect is also very atmospheric. In the process of laying tiles, gaps need to be left between adjacent tiles. In the past, during the construction process, gypsum powder and other materials were filled in the gaps, but it is easy to loose and fall off and accumulate stains after a long time; now more and more Filling with beauty agent, after filling with beauty agent, it is more beautiful and can be stable for a long time. [0003] General beautifying agents are mainly composed of epoxy resin and pigments. They are used for plum blossoms in the gaps of tile...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Applications(China)
IPC IPC(8): C09J163/02C09J11/04
CPCC09J163/00C09J11/04C08K2201/011C08L2205/025C08L63/00C08K13/04C08K5/05C08K3/042C08K3/346C08K7/26
Inventor 李全涛李应林庹斌峰游军陈天有余海斌徐祖顺
Owner 杭州华圩新材料科技有限公司