Cement paste toughening agent and application of cement paste toughening agent in preparation of cementing flexible cement paste
A technology of cement slurry and toughening agent, applied in the field of oil and gas well cementing, can solve the problem of increasing the bonding force between rubber powder and cementing cement stone interface, affecting the later mechanical properties of modified composite materials, and decreasing the hydrophilicity of rubber powder. problems, to achieve the effect of adjustable thickening time, low processing cost and strong production controllability
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0032] 1. Preparation of cement slurry toughening agent:
[0033] (1) Cleaning of rubber powder: Put the rubber powder in a glass container and spread it evenly, put it in the cavity of the plasma processor, turn on the power, turn on the vacuum pump, and when the vacuum in the cavity reaches below 10Pa, open the flow valve and put When the gas is processed, when the flow rate reaches the set value, turn on the high-frequency power supply and start discharging;
[0034] (2) Activation and etching of rubber powder: continue to process the cleaned rubber powder with the method described in step (1);
[0035] (3) Grafting of rubber powder: place the activated and etched rubber powder in the plasma grafting equipment, put in the grafting gas under vacuum conditions, and turn on the high-frequency power supply when the flow rate reaches the set value Start discharging.
[0036] The relevant parameters are as follows:
[0037]
[0038]
[0039] 2. Preparation of flexible ce...
Embodiment 2
[0042] 1. Preparation of cement slurry toughening agent:
[0043] Steps as described in Example 1, relevant parameters are as follows:
[0044]
[0045] 2. Preparation of flexible cement slurry for well cementing:
[0046] Weigh 100 parts by weight of oil well cement, 20 parts by weight of modified rubber powder, 10 parts by weight of micro silicon, and dry mix 40 parts by weight of barite into dry powder, measure 35 parts by weight of water, weigh 2 parts by weight of sodium hexametaphosphate, 3 parts by weight of 2-acrylamide-2-methylpropanesulfonic acid, 2.5 parts by weight of citric acid, and 0.5 parts by weight of tributyl phosphate were dissolved in water. Then, put the aqueous solution in the mixing container, the stirrer rotates at a low speed (4000±200 rpm), and add the mixed dry powder within 15 seconds, cover the lid of the stirrer, and turn it at a high speed (12000±200 rpm). 500 rev / min) and continue stirring for 35 seconds to obtain flexible cement slurry fo...
Embodiment 3
[0048] 1. Preparation of cement slurry toughening agent:
[0049] Steps as described in Example 1, relevant parameters are as follows:
[0050] Rubber powder mesh
80 mesh
purge gas type
Cleaning gas flow
0.1L / min
cleaning power
220W
cleaning time
45s
Activated etching gas type
Activation etch gas flow
0.1L / min
Activation etching power
280W
Activation etch time
70s
grafting gas type
ethanol vapor
grafting gas flow
1L / min
grafting power
50W
grafting time
195s
[0051] 2. Preparation of flexible cement slurry for well cementing:
[0052] Take 100 parts by weight of oil well cement, 18 parts by weight of modified rubber powder, 12 parts by weight of microsilicon, and dry mix 35 parts by weight of barite into dry powder, measure 65 parts by weight of water, weigh 1.7 parts by weight of sodium hexametaphosphate, 0.5 parts ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com