3-vinylamino-2-hydroxypropyltrimethylammonium chloride copolymer and its preparation and application

A technology based on hydroxypropyltrimethylammonium chloride and vinylamine, which is applied in chemical instruments and methods, textiles and papermaking, and special treatment targets, etc. It can solve the problem of limited increase in fiber molecular level bonding area, slow fiber response, and economical Poor efficiency and other problems, to achieve the effect of easy access to raw materials, short production cycle, and improved cleanliness

Active Publication Date: 2018-07-17
FUZHOU UNIV
View PDF7 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The traditional cationic sizing agent usually uses starch, but the general starch-based papermaking strengthening agent has limited improvement in the bonding area at the fiber molecular level, and consumes a lot of food, resulting in poor economic benefits. [5]
Traditional sizing agent emulsions use cationic starch as emulsifier and stabilizer, but the retention rate of this type of emulsion on fibers is relatively low, the reaction with fibers is relatively slow, and the required sizing time is long [6]

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • 3-vinylamino-2-hydroxypropyltrimethylammonium chloride copolymer and its preparation and application
  • 3-vinylamino-2-hydroxypropyltrimethylammonium chloride copolymer and its preparation and application
  • 3-vinylamino-2-hydroxypropyltrimethylammonium chloride copolymer and its preparation and application

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0073] 1. The raw material group used in this embodiment is as follows (unit: kilogram)

[0074] Acrylamide monomer: 22.0 kg,

[0075] Chain transfer agent (urea): 5.0 kg,

[0076] Complexing agent (EDTA2Na): 2.0 kg,

[0077] Initiator (a mixture of ammonium persulfate and potassium persulfate, the mass ratio is 1:1): 2.0 kg,

[0078] Sodium hydroxide: 121.0 kg,

[0079] Sodium hypochlorite (10%): 250.0 kg,

[0080] Epichlorohydrin: 5.0 kg,

[0081] Trimethylamine: 3.0 kg,

[0082] Distilled water: 590.0 kg;

[0083] 2. Preparation process steps and parameters

[0084] (1) Dissolve acrylamide monomer in 215.0 kg of distilled water, add chain transfer agent, complexing agent, and initiator, stir for 15 minutes in a water bath at 40°C, and let stand for 20 minutes;

[0085] (2) At 10°C, add 12.0 kg of sodium hydroxide while stirring to make it evenly mixed, then slowly add sodium hypochlorite, stir and react for 2 hours, then add 109.0 kg of sodium hydroxide, and stir fo...

Embodiment 2

[0088] 1. The raw material group used in this embodiment is as follows (unit: kilogram)

[0089] Acrylamide monomer: 22.0 kg,

[0090] Chain transfer agent (urea): 5.0 kg,

[0091]Complexing agent (EDTA2Na): 2.0 kg,

[0092] Initiator (ammonium persulfate): 1.0 kg,

[0093] Sodium hydroxide: 121.0 kg,

[0094] Sodium hypochlorite (10%): 224.0 kg,

[0095] Epichlorohydrin: 6.0 kg,

[0096] Trimethylamine: 4.0 kg,

[0097] Distilled water: 615.0 kg;

[0098] 2. Preparation process steps and parameters

[0099] (1) Dissolve acrylamide monomer in 215.0 kg of distilled water, add chain transfer agent, complexing agent, and initiator, stir for 15 minutes in a water bath at 40°C, and let stand for 20 minutes;

[0100] (2) At 5°C, add 12.0 kg of sodium hydroxide while stirring to make it evenly mixed, then slowly add sodium hypochlorite, stir and react for 2 hours, then add 109.0 kg of sodium hydroxide, and stir for 4 hours.

[0101] (3) Add epichlorohydrin dropwise at 30°C, ...

Embodiment 3

[0103] 1. The raw material group used in this embodiment is as follows (unit: kilogram)

[0104] Acrylamide monomer: 22.0 kg,

[0105] Chain transfer agent (mixture of urea and isopropanol, the mass ratio is 1:1): 5.0 kg,

[0106] Complexing agent (a mixture of EDTA2Na and HEDTA, the mass ratio is 1:1): 2.0 kg,

[0107] Initiator (a mixture of ammonium persulfate and potassium persulfate, the mass ratio is 1:1): 3.0 kg,

[0108] Sodium hydroxide: 150.0 kg,

[0109] Sodium hypochlorite (10%): 200.0 kg,

[0110] Epichlorohydrin: 6.0 kg,

[0111] Trimethylamine: 4.0 kg,

[0112] Distilled water: 608.0 kg;

[0113] 2. Preparation process steps and parameters

[0114] (1) Dissolve acrylamide monomer in 180.0 kg of distilled water, add chain transfer agent, complexing agent, and initiator, stir for 15 minutes in a water bath at 40°C, and let stand for 20 minutes;

[0115] (2) At 15°C, add 20.0 kg of sodium hydroxide while stirring to make it evenly mixed, then slowly add sod...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
solid contentaaaaaaaaaa
degree of polymerizationaaaaaaaaaa
quality scoreaaaaaaaaaa
Login to view more

Abstract

The invention discloses 3-vinylamino-2-hydroxypropyltrimethylammonium chloride copolymer and preparation and application thereof.The preparation includes: placing acrylamide monomer and distilled water in a N2 protected reactor, adding a chain transfer agent, a complexing agent and an initiator, stirring at 30-70 DEG C for 10-30 min, standing for 10-30 min, cooling to 10-15 DEG C, adding sodium hydroxide, stirring well and then adding sodium hydrochloride slowly, reacting for 1-3 h, adding sodium hydroxide, reacting for 2-4 h, dropwise adding epichlorohydrin, reacting for 0.1-0.5 h, heating to 50-90 DEG C, reacting for 1-3 h, dropwise adding trimethylamine aqueous solution slowly, and reacting for 2-5 h and then cooling to normal temperature to obtain the 3-vinylamino-2-hydroxypropyltrimethylammonium chloride copolymer; the copolymer is light yellow thick liquid, > / =13% in solid content, 9-10 in pH, 80-100 in degree of polymerization and higher than 60% in amination degree, and is useful as a paper enhancer, a paper sizing agent, a water treating agent and the like.The preparation process is simple, production materials are easy to obtain, a production cycle is short, reacting is mild, and invention is convenient for industrial large-scale production and has a promising application prospect.

Description

technical field [0001] The invention belongs to the fields of fine chemicals, environment-friendly materials, papermaking additives and water treatment agents, and specifically relates to a 3-vinylamino-2-hydroxypropyl trimethylammonium chloride copolymer and its preparation and application. Background technique [0002] With the improvement of consumption level, people have higher and higher requirements for paper grade and quality. How to improve the strength of paper to meet people's needs is the direction that people have been studying. We can increase the ratio of long fibers by beating and use reinforcing agents to enhance the strength of paper. Among them, there are many defects in the two methods of beating and the ratio of long fibers, such as large power consumption and low water drainage. , tearing becomes weaker, etc., and paper additives are favored by people because they do not have the above problems [1] . [0003] Paper sizing agents can improve the appeara...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Patents(China)
IPC IPC(8): C08F120/56C08F8/44D21H17/45D21H19/58D21H21/16D21H21/20C02F1/56
CPCC02F1/56C02F2303/22C08F8/44C08F120/56D21H17/45D21H19/58D21H21/16D21H21/20
Inventor 刘明华林立刘以凡
Owner FUZHOU UNIV
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products