Method for preparing multifunctional aquatic water modifier
A technology for aquaculture water body and improver, which is applied in the field of preparation of aquaculture water body improver, which can solve the problems of no significant benefit, no insecticidal function, unstable water transfer effect, etc., to increase the species and quantity of planktonic organisms, Shorten the reproductive cycle and benefit the growth
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0018] The preparation method of the multifunctional aquaculture water body improver comprises the following specific steps:
[0019] 1) Mix 14 parts of weathered coal, 7 parts of alkali metal silicate and 2 parts of deionized water, and react at a temperature of 70°C for 50 minutes to obtain a humic acid solution. The prepared humic acid solution is weakly alkaline, which can make The silicic acid and humic acid in the solution are not easy to settle, which can effectively reduce the accumulation of the modifier in the water body. At the same time, it contains silicon ions, which have the nutritional value of silicon fertilizer. It not only provides nutrients such as planktonic organic matter and silicon, but also It has the function of cultivating algae and cultivating algae;
[0020] 2) Dissolve humic acid in 5% NaOH solution, add to the reaction device and heat for 10 minutes, then add polyethylene glycol with 5% humic acid weight, under nitrogen protection, temperature 12...
Embodiment 2
[0024] The preparation method of the multifunctional aquaculture water body improver comprises the following specific steps:
[0025] 1) Mix 14 parts of weathered coal, 7 parts of alkali metal silicate and 2 parts of deionized water, and react at a temperature of 90°C for 70 minutes to obtain a humic acid solution;
[0026] 2) Dissolve humic acid in 8% NaOH solution, add to the reaction device and heat for 15 minutes, then add polyethylene glycol with 7% humic acid weight, under nitrogen protection, temperature 135°C, heat reaction for 1.5 hours to obtain grafted Humic acid modified by copolymerization reaction;
[0027] 3) Add 0.12 parts of Al 2 (SO 4 ) 3 , 0.1 parts of ClO 2 Add 0.08 parts of 1-hydroxydodecyltrimethylammonium bromide to bentonite, and react for 40 minutes at a pH value of 9.0, adjust the pH to 4.5, place it in a microwave oven with a power of 1500W, and heat it by irradiation 20min, synthetic inorganic-organic bentonite, above-mentioned ClO 2 ionized H...
Embodiment 3
[0030] The preparation method of the multifunctional aquaculture water body improver comprises the following specific steps:
[0031] 1) Mix 14 parts of weathered coal, 7 parts of alkali metal silicate and 2 parts of deionized water, and react at a temperature of 80°C for 60 minutes to obtain a humic acid solution;
[0032] 2) Dissolve humic acid in 10% NaOH solution, add to the reaction device and heat for 20 minutes, then add polyethylene glycol with 9% humic acid weight, under nitrogen protection, temperature 150°C, heat reaction for 2 hours, and obtain graft copolymerized Reaction-modified humic acid, the above-mentioned polyethylene glycol contains 0.08% ethyl propionate by weight, and the added ethyl propionate can assist heating to destroy the structure of polyethylene glycol, making the polyethylene glycol part weak The bond is broken faster, the internal hydrophilic polar group is exposed to the surface of the molecule, and quickly dissolves in water, thereby accelera...