Anti-rainwater dust suppressant and preparation method thereof
A dust suppressant and anti-rain technology, which is applied in chemical instruments and methods, and other chemical processes, can solve the problems of poor dust suppression effect and slow film formation speed, and achieves improved rain erosion resistance, improved film formation, and excellent cohesive effect
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0038] This embodiment provides a rainproof and dust-suppressant agent and a preparation method thereof, wherein the rain-proof and dust-suppressant agent comprises raw materials of the following weight:
[0039] 0.2kg water-soluble alkyd resin; 0.5kg organic bentonite; 0.8kg water-soluble starch; 4kg glycerol; 0.1kg perfluorohexylethylmethyldimethoxysilane; 0.2kg styrene-acrylamide copolymer; kg polysiloxane-polyalkoxyether copolymer; 2 kg sodium alginate and 100 kg water.
[0040] The preparation method of above-mentioned rainproof dust suppression agent is as follows:
[0041] Weigh 0.2 kg of water-soluble alkyd resin and add it to 40 kg of water to swell, stir at room temperature for 15 minutes at a stirring rate of 900 rpm to dissolve, and obtain a water-soluble polymer;
[0042] Weigh 0.5 kg of organic bentonite and 0.8 kg of water-soluble starch into 20 kg of water, stir and mix at room temperature at 1500 rpm for 10 minutes to obtain a mixed aqueous solution A;
[00...
Embodiment 2
[0046] This embodiment provides a rainproof and dust-suppressant agent and a preparation method thereof, wherein the rain-proof and dust-suppressant agent comprises raw materials of the following weight:
[0047] 8kg water-soluble alkyd resin; 0.1kg organic bentonite; 0.6kg water-soluble starch; 3kg glycerol; 3kg butylene glycol; 1kg (3,3,3-trifluoropropyl) dichloromethylsilane; 0.1kg benzene Ethylene-acrylamide copolymer; 0.4 kg polysiloxane-polyalkoxyether copolymer; 4 kg sodium alginate and 110 kg water.
[0048] The preparation method of above-mentioned rainproof dust suppression agent is as follows:
[0049] Weigh 8 kg of water-soluble alkyd resin and add it to 35 kg of water to swell, stir at room temperature for 20 minutes at a stirring speed of 800 rpm to dissolve, and obtain a water-soluble polymer;
[0050] Weigh 0.1 kg of organic bentonite and 0.6 kg of water-soluble starch into 30 kg of water, stir and mix at room temperature at 1350 rpm for 15 minutes to obtain a...
Embodiment 3
[0054] This embodiment provides a rainproof and dust-suppressant agent and a preparation method thereof, wherein the rain-proof and dust-suppressant agent comprises raw materials of the following weight:
[0055] 2kg water-soluble acrylic resin; 0.2kg organic bentonite; 1kg water-soluble starch; 1kg glycerol; 2kg sorbitol; 2kg perfluorohexylethylmethyldimethoxysilane; 0.4 kg polysiloxane-polyalkoxy ether copolymer; 3 kg sodium alginate and 140 kg water.
[0056] The preparation method of above-mentioned rainproof dust suppression agent is as follows:
[0057] Weigh 2 kg of water-soluble acrylic resin and add it to 40 kg of water to swell, stir at room temperature for 25 minutes at a stirring rate of 600 rpm to dissolve, and obtain a water-soluble polymer;
[0058] Weigh 0.2 kg of organic bentonite and 1 kg of water-soluble starch into 50 kg of water, stir and mix at room temperature at 1300 rpm for 15 minutes to obtain a mixed aqueous solution A;
[0059] Weigh 1kg glycerol,...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com