Plastering mortar using high-volume slag and preparation method thereof
A technology for plastering mortar and bottom slag, which is applied in sustainable waste treatment, solid waste management, climate sustainability, etc. The increase in water consumption of mortar and other problems can achieve the effect of saving equipment, reducing wet bulk density and saving consumption.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0032] (1) Dry the river sand and furnace bottom slag respectively until the moisture content is lower than 0.2%, and sieve out the large particles above 3mm before putting them into the warehouse for use;
[0033] (2) 100kg of plastering mortar masterbatch is prepared, and the raw material quality of each component is:
[0034] Powdered naphthalene-based water reducer 8.2kg,
[0035] Fatty alcohol sulfate anionic surfactant 0.63kg,
[0036] Cellulose ether 3.1kg,
[0037] Stick clay 15.3kg,
[0038] Class I fly ash 72.77kg.
[0039] Put the above-mentioned raw materials into the mixer, mix them thoroughly for 4 minutes, and put them into the additive warehouse for use after mixing evenly;
[0040] (3) Prepare 100kg of dry-mixed plastering mortar DPM5.0 finished product, and the raw material quality of each component is:
[0041] Ordinary Portland cement 17.2kg,
[0042] Class I fly ash 7.1kg,
[0043] River sand 49.8kg,
[0044] Bottom slag 23.8kg,
[0045] Plasterin...
Embodiment 2
[0048] (1) Dry the river sand and furnace bottom slag respectively until the moisture content is lower than 0.2%, and sieve out the large particles above 3mm before putting them into the warehouse for use;
[0049] (2) 100kg of plastering mortar masterbatch is prepared, and the raw material quality of each component is:
[0050] Powdered naphthalene-based water reducer 10.3kg,
[0051] Fatty alcohol sulfate anionic surfactant 0.59kg,
[0052] Polyacrylamide 4.0kg,
[0053] Stick clay 19.2kg,
[0054] Class I fly ash 65.91kg.
[0055] Put the above raw materials into the mixer, mix thoroughly for 5 minutes, mix well and put them into the additive warehouse for use;
[0056] (3) Prepare 100kg of dry-mixed plastering mortar DPM5.0 finished product, and the raw material quality of each component is:
[0057] Ordinary Portland cement 16.5kg,
[0058] Class I fly ash 6.7kg,
[0059] River sand 56.9kg,
[0060] Bottom slag 18.3kg,
[0061] Plastering mortar masterbatch 1.6kg...
Embodiment 3
[0064] (1) Dry the river sand and furnace bottom slag respectively until the moisture content is lower than 0.2%, and sieve out the large particles above 3mm before putting them into the warehouse for use;
[0065] (2) 100kg of plastering mortar masterbatch is prepared, and the raw material quality of each component is:
[0066] Powdered melamine-based water reducer 8.7kg,
[0067] Fatty alcohol sulfate anionic surfactant 0.54kg,
[0068] Polyvinyl alcohol 3.5kg,
[0069] Bentonite 15.8kg,
[0070] Stone powder 71.46kg.
[0071] Put the above raw materials into the mixer, mix thoroughly for 5 minutes, mix well and put them into the additive warehouse for use;
[0072] (3) Prepare 100kg of dry-mixed plastering mortar DPM7.5 finished product, and the raw material quality of each component is:
[0073] Portland cement 18.3kg,
[0074] Class I fly ash 7.3kg,
[0075] Machine-made sand 51.8kg,
[0076] Bottom slag 20.6kg,
[0077] Plastering mortar masterbatch 2.0kg.
[0...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com