Production method of lead-free ceramic-simulating glass winebottles
A production method and glass technology, applied in glass production, glass molding, glass blowing, etc., can solve problems such as headache, dizziness, fatigue, drowsiness, constipation, sore limbs, permanent disability, and inattention, and achieve The effect of convenient source of raw materials, low production cost and simple process
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0016] Crushed glass accounting for 29% of the total, quartz sand accounting for 34% of the total, soda ash accounting for 10% of the total, albite accounting for 15% of the total, calcite accounting for 8% of the total, 0.1% of the total amount of sodium sulfate and 3.9% of the total amount of sodium fluorosilicate are sent to the blender to mix evenly to obtain a mixture, and the mixture is sent to the kiln through the conveyor; the coal is sent to the boiler Combustion, the 540°C gas obtained by combustion is sent to the kiln through the gas transmission equipment, and is sealed and burned in the kiln, so that the temperature of the mixture reaches 1560°C, and maintains this temperature for 28 hours, so that the mixture reaches a molten state and obtains lead-free Imitation porcelain glass melt, if the porcelain degree of the product measured at this time is not enough, the proportion of quartz sand can be appropriately reduced, and the proportion of sodium fluorosilicate ca...
Embodiment 2
[0018] cullet accounting for 30% of the total, quartz sand accounting for 33% of the total, soda ash accounting for 10% of the total, albite accounting for 15% of the total, calcite accounting for 8% of the total, 0.1% of the total amount of sodium sulfate and 3.9% of the total amount of sodium fluorosilicate are sent to the blender to mix evenly to obtain a mixture, and the mixture is sent to the kiln through the conveyor; the coal is sent to the boiler Combustion, the 550°C gas obtained by combustion is sent to the kiln through the gas transmission equipment, and is sealed and burned in the kiln, so that the temperature of the mixture reaches 1555°C, and maintains this temperature for 30 hours, so that the mixture reaches a molten state and obtains lead-free Imitation porcelain glass melt, if the porcelain degree of the product measured at this time is not enough, the proportion of quartz sand can be appropriately reduced, and the proportion of sodium fluorosilicate can be in...
Embodiment 3
[0020] Culled glass accounting for 31% of the total, quartz sand accounting for 32% of the total, soda ash accounting for 10% of the total, albite accounting for 15% of the total, calcite accounting for 8% of the total, 0.1% of the total amount of sodium sulfate and 3.9% of the total amount of sodium fluorosilicate are sent to the blender to mix evenly to obtain a mixture, and the mixture is sent to the kiln through the conveyor; the coal is sent to the boiler Combustion, the 560°C gas obtained by combustion is sent to the kiln through the gas transmission equipment, and is sealed and burned in the kiln, so that the temperature of the mixture reaches 1550°C, and maintains this temperature for 32 hours, so that the mixture reaches a molten state and obtains lead-free Imitation porcelain glass melt, if the porcelain degree of the product measured at this time is not enough, the proportion of quartz sand can be appropriately reduced, and the proportion of sodium fluorosilicate can...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com