Low-temperature-resistant door/window sealing strip and preparation method thereof

A technology of sealing strip and low temperature resistance, applied in the field of building materials, can solve the problems of cracking, easy dust absorption, physical and mechanical properties deterioration, etc., achieve high-strength aging resistance, good aging resistance, and reduce elongation at break Effect

Active Publication Date: 2015-06-17
SUZHOU TONGMING MACHINERY
View PDF7 Cites 7 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0002]With the improvement of people's quality of life, the demand for living space also increases, and the improvement of building quality requirements is particularly prominent; in the process of building doors and windows Among them, the investment of sealing strips accounts for a small proportion, but its role cannot be ignored. The key to doors and windows lies in the sealing, in which the sealing strips play a pivotal role; the material of sealing strips on the market is generally modified by PVC, rubber As well as fibers and fluff, the small molecule plasticizer in the modified PVC is easy to migrate to the surface of the product, resulting in poor elasticity of the sealing strip and hardening of the material, thereby affecting the sealing performance of doors and windows; rubber sealing strips, In the rubber production process, there are weaknesses of high energy consumption and heavy pollution. After being used as sealing strips, some small molecule additives also have defects such as strong migration and poor elasticity, and are more harmful to the human body. Large, at present, the most common rubber type is EPDM (ethylene propylene diene monomer) sealing strip, although EPDM itself has good heat resistance
Chemical medium resistance, water resistance, etc., but as an organic polymer material, due to the combined effects of external environmental factors (such as light, heat, oxygen, and corrosive media, etc.) during use, it will cause changes in physical and mechanical properties. Gradually deteriorate until the final loss of use value, the surface is cracked, sticky, hardened, softened, powdered, discolored and moldy, etc., which will bring great inconvenience to people's normal life and office
[0003] However, the existing sealing strips of medium fiber and fluff are easy to absorb dust, have low strength, low elasticity, and poor sealing performance. Therefore, a kind of door and window that can overcome the above defects is developed. Sealing strips become a technical problem to be solved urgently by those skilled in the art

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0058] This embodiment provides a low-temperature-resistant door and window sealing strip. The door and window sealing strip is composed of two components A and B mixed, and mixed according to the mass ratio of A:B=2:1, wherein:

[0059] Component A includes the following components in parts by mass:

[0060] Modified EPDM rubber: 61 parts, white carbon black: 9 parts, silane coupling agent: 10 parts, dimethyl silicone oil: 10 parts, vulcanizing agent BIBP: 9 parts, petroleum softener: 7 parts, ten Sodium dialkylbenzenesulfonate: 10 parts;

[0061] Component B includes the following components in parts by mass:

[0062] SBR: 35 parts, calcium carbonate: 10 parts, propylene glycol: 8 parts, antioxidant 1010: 2 parts, antioxidant 168: 3 parts;

[0063] Among them: modified EPDM rubber includes the following components in parts by mass:

[0064] EPDM rubber: 60 parts, organic montmorillonite: 20 parts, carbon black: 35 parts, zinc oxide: 9 parts, stearic acid: 8 parts, sulfur:...

Embodiment 2

[0083] This embodiment provides a low-temperature-resistant door and window sealing strip. The door and window sealing strip is composed of two components A and B mixed, and mixed according to the mass ratio of A:B=2:1, wherein:

[0084] Component A includes the following components in parts by mass:

[0085] Modified EPDM rubber: 50 parts, white carbon black: 10 parts, silane coupling agent: 8 parts, dimethyl silicone oil: 8 parts, vulcanizing agent DPTT: 10 parts, pine oil softener: 9 parts, Sodium dioctyl succinate: 15 parts

[0086] Component B includes the following components in parts by mass:

[0087] SBR: 30 parts, talcum powder: 9 parts, diethanolamine: 7 parts, antioxidant 1010: 2 parts, antioxidant 168: 3 parts;

[0088] Among them: modified EPDM rubber includes the following components in parts by mass:

[0089] EPDM rubber: 70 parts, organic montmorillonite: 10 parts, carbon black: 30 parts, zinc oxide: 5 parts, stearic acid: 5 parts, sulfur: 8 parts, accelerat...

Embodiment 3

[0108] This embodiment provides a low-temperature-resistant door and window sealing strip. The door and window sealing strip is composed of two components A and B mixed, and mixed according to the mass ratio of A:B=2:1, wherein:

[0109] Component A includes the following components in parts by mass:

[0110] Modified EPDM rubber: 65 parts, white carbon black: 8 parts, silane coupling agent: 7 parts, dimethyl silicone oil: 6 parts, vulcanizing agent BIBP: 8 parts, fatty oil softener: 10 parts, Sodium dodecylbenzenesulfonate: 12 parts

[0111] Component B includes the following components in parts by mass:

[0112] SBR: 30 parts, diatomaceous earth: 9 parts, 1,4-butanediol: 7 parts, antioxidant 1010: 2 parts, antioxidant 168: 3 parts;

[0113] Among them: modified EPDM rubber includes the following components in parts by mass:

[0114] EPDM rubber: 65 parts, organic montmorillonite: 15 parts, carbon black: 40 parts, zinc oxide: 7 parts, stearic acid: 10 parts, sulfur: 5 part...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

No PUM Login to View More

Abstract

The invention discloses a low-temperature-resistant door / window sealing strip which is formed by mixing a component A and a component B in a mass ratio of 2:1. The component A comprises modified ethylene propylene diene monomer rubber, a filler, a coupling agent, a plasticizer, a vulcanizing agent, a softening agent and an activator. The component B comprises the following components in parts by mass: styrene-butadiene rubber, a filler, a chain extender and an antioxidant. The invention also discloses a preparation method of the low-temperature-resistant door / window sealing strip. The preparation method is simple to operate and easy to implement, and has the advantage of low cost. The door / window sealing strip has the advantages of favorable cold resistance, favorable heat resistance, favorable aging resistance, favorable sealing property and longer service life.

Description

technical field [0001] The invention relates to a sealing strip, in particular to a sealing strip on doors and windows and a preparation method thereof, belonging to the technical field of building materials. Background technique [0002] With the improvement of people's quality of life, the demand for living space also increases, among which the improvement of building quality requirements is particularly prominent; in the process of building doors and windows, the investment of sealing strips accounts for a small proportion, but its role is significant. It cannot be ignored that the key of doors and windows lies in sealing, among which the sealing strip plays a pivotal role; the sealing strip materials on the market are generally PVC modified, rubber, fiber, and fluff. Molecular plasticizers are easy to migrate to the surface of the product, resulting in poor elasticity of the sealing strip and hardening of the material, thereby affecting the sealing performance of doors a...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
IPC IPC(8): C08L23/16C08L9/06C08K13/06C08K9/06C08K3/34C08K3/04C08K3/22C08K5/09C08K5/42C08K3/36
CPCC08L23/16C08L2201/08C08L2205/03C08L2205/035C08L9/06C08L83/04C08K13/06C08K9/06C08K3/36C08K3/346C08K3/04C08K2003/2296C08K5/09C08K3/06C08K2003/265C08K5/053C08K5/1345C08K5/526C08L91/00C08K3/34C08K5/17
Inventor 黄龙海黄瑶琼吴磊
Owner SUZHOU TONGMING MACHINERY
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products