New method for recovering nickel, cobalt, iron, silicon and magnesium from low-grade laterite-nickel ore

A laterite nickel ore, low-grade technology, applied in the field of silicon and magnesium, iron, wet leaching process, recovery of nickel and cobalt, can solve the problems of long process cycle, long leaching time, rising production cost, etc., to achieve operation and maintenance Simple, low investment and operating costs

Inactive Publication Date: 2015-07-29
JINCHUAN GROUP LIMITED
View PDF13 Cites 1 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

For example, the invention patent with the publication number CN101273146A proposes a two-step normal-pressure leaching method for simultaneously extracting limonite and saprolite or leaching limonite and then saprolite ore. This method has the advantage of not using an autoclave. However, in the process described in the application, it is proposed that when the leaching solution is treated to remove Fe and / or Al, it is necessary to add a neutralizing agent to neutralize the residual acid in the leaching solution, so that most of the iron is in the form of ferric hydroxide Deposition, which will cause loss of valuable elements such as nickel and cobalt and difficulty in slurry filtration
Another example is the patent of invention whose publication number is CN101541985A, which proposes a method for leaching a mixture of limonite and saprolite at normal pressure, but its iron precipitation product is jarosite, which contains sulfate radicals, so It will increase the acid consumption of the leaching process; and jarosite is a thermodynamically unstable compound, which will release sulfuric acid during accumulation and storage, thereby causing environmental pollution
Another example is the invention patent of CN101006190A with the publication number, which proposes a method for treating the mixture of limonite and saprolite ore with concentrated acid and then leaching nickel and cobalt with water. The iron deposit produced by this method is except jarosite. Ferric oxide or hydroxide, but the leaching time of this application needs 12-48h, and the leaching time is longer, resulting in a longer process cycle and increased production costs
[0018] In short, in the above-mentioned invention patents of lateritic nickel ore wet smelting, the disadvantages of the high-pressure acid leaching (HPAL) process and the improved high-pressure acid leaching process are: complex high-temperature, high-pressure autoclaves and related equipment are required, and their installation and Both are expensive to maintain; the HPAL process consumes more sulfuric acid than is required to stoichiometrically dissolve the non-ferrous components of the ore; the HPAL process is limited to processing mainly limonite-type feedstock; the HPAL process operates at high pressure The kettle is prone to fouling, and needs to be shut down regularly for cleaning, and the operating rate is low
The disadvantages of the atmospheric pressure acid leaching process and the improved atmospheric pressure acid leaching process are: high sulfuric acid consumption; low nickel and cobalt leaching rates; long reaction time and huge equipment required
The common disadvantage of high-pressure acid leaching including improved high-pressure acid leaching process and atmospheric pressure acid leaching process including improved atmospheric pressure acid leaching process is that the amount of leaching slag is large, and it is a mixed slag of silicon and iron, so that the main component of laterite ore, iron, cannot Economical and effective development and utilization
Although the invention patent of CN102206749A mentions the recycling of leaching slag, since the silicon dioxide, iron oxide, goethite, etc. Simple magnetic separation and other methods separate them, so the economic benefits of the development and utilization of the above-mentioned leaching slag are very poor, and they can only be treated as waste solids, and even the leaching slag with a low nickel leaching rate must be treated as hazardous waste.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • New method for recovering nickel, cobalt, iron, silicon and magnesium from low-grade laterite-nickel ore

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0043] Take 500Kg (dry basis) and grind to 80 mesh 2 # Add 500Kg water to the high-silicon magnesium ore to make high-silicon magnesium slurry, and prepare 500Kg of concentrated sulfuric acid (98%). Use the mortar pump and the concentrated sulfuric acid pump to strictly control the flow rate to add the high-silicon magnesium slurry and concentrated sulfuric acid into the steel-lined alloy reaction tank for reaction. The total reaction time is 10 minutes.

[0044] After cooling down, the reaction material of the crisp and loose honeycomb solid paste is simply broken and poured into a water immersion tank, and 1500Kg of water is added, and stirred for about 30 minutes. Pump the water-soluble slurry into a plate and frame filter press for solid-liquid separation and filter residue washing to obtain 205Kg (dry) atmospheric acid leaching filter residue (A1), 1450L atmospheric pressure acid leaching filtrate (B1) and 1150L washing liquid (E1) . The components of atmospheric acid ...

Embodiment 2

[0055] Take 500Kg (dry basis) and grind to 80 mesh 5 # Add 500Kg water to the high-silicon magnesium ore to make high-silicon magnesium slurry, and prepare 500Kg of concentrated sulfuric acid (98%). Use the mortar pump and the concentrated sulfuric acid pump to strictly control the flow rate to add the high-silicon magnesium slurry and concentrated sulfuric acid into the steel-lined alloy reaction tank for reaction. The total reaction time is 10 minutes.

[0056] After cooling down, the reaction material of the crisp and loose honeycomb solid paste is simply broken and poured into a water immersion tank, and 1500Kg of water is added, and stirred for about 30 minutes. Pump the water-soluble slurry into a plate and frame filter press for solid-liquid separation and filter residue washing to obtain 230Kg (dry) atmospheric acid leaching filter residue (A2), 1400L atmospheric pressure acid leaching filtrate (B2) and 1180L washing liquid (E2) . The components of atmospheric acid le...

Embodiment 3

[0067] The normal-pressure acid leaching stage of the present embodiment is the same as that of Example 1, and 3 Xinka low-silicon magnesium ore was replaced by 6 # Indonesian low silicon magnesium ore.

[0068] Take 30Kg (dry) 6 # Low-silicon magnesium ore, add 60L of washing liquid (E1) to make low-silicon magnesium slurry, heat it to 95°C and move it into the circulation tank of the pressurized pipeline reactor, and then add 95°C Atmospheric pressure acid leaching filtrate (B1) 30L. After sealing the circulation tank, turn on the booster pump, the pressure is not higher than 3.0Mpa, and at the same time turn on the heat conduction oil heating device of the pressurized pipeline reactor, control the temperature and heat, when the temperature rises to 225°C, continue to heat at a constant temperature for 60 minutes, then stop heating and cool down Cool down. The final pH value after material reaction is 0.8. After cooling down to 85°C, remove the reaction slurry from the...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

A new method for recovering nickel, cobalt, iron, silicon and magnesium from low-grade laterite-nickel ore is disclosed. The new method comprises the following steps: washing and grading; carrying out a reaction by adding enough concentrated sulfuric acid into high-silica magnesite ore pulp, and carrying out solid-liquid separation to obtain atmospheric pressure leaching residues and an atmospheric pressure leaching agent; adding the atmospheric pressure leaching agent and low-silica magnesite high-iron ore pulp in proportion into a tubular reactor and carrying out pressure leaching; carrying out solid-liquid separation; purifying and precipitating a pressure leaching filtrate by the use of magnesium oxide and filtering to obtain nickel hydroxide (cobalt hydroxide); carrying out evaporative crystallization on a nickel-precipitated liquid so as to obtain magnesium sulfate heptahydrate; washing and drying pressure leaching residues to obtain fine iron powder; and screening the atmospheric pressure leaching residues to obtain a silicon dioxide product and building sand. The method has advantages as follows: wide application range of lateritic ore; high Ni-Co leaching rate; small atmospheric pressure leaching equipment; short time; high efficiency; and low sulfuric acid consumption. As the middle and low pressure tubular reactor is adopted for pressure leaching, the defect that autoclave equipment is expensive and easy to scale is avoided. Main components of ore, such as iron, magnesium and part of silicon, can be recovered economically and effectively. The amount of waste residues is low, and the waste residues can be utilized effectively.

Description

technical field [0001] The invention belongs to the field of metallurgy, is a wet leaching process, and relates to a new method for recovering nickel, cobalt, iron, silicon and magnesium from low-grade laterite nickel ore. Background technique [0002] Laterite ore is a nickel oxide ore formed by nickel-bearing peridotite after large-scale long-term weathering and leaching metamorphism in tropical or subtropical regions. Due to differences in geographical location, climatic conditions and weathering degrees, the types of laterite ore around the world are not completely the same . [0003] The weathering process generally produces layered deposits in which complete or most complete weathering is present near the surface, gradually becoming less weathered with increasing depth, and finally terminating at some deeper depth as unweathered rock. [0004] Highly regolithed layers typically have most of the nickel they contain finely distributed in finely divided goethite grains....

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C22B23/00C01B33/113C01D5/10
CPCY02P10/20
Inventor 杨志强刘玉强王少华陈学安沙滨杜昊王纪华姚菲唐金贺小红
Owner JINCHUAN GROUP LIMITED
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products