A positive electrode material, high-nickel technology, applied in the direction of positive electrode, active material electrode, electrical components, etc., can solve the problems of poor cycle performance and electrochemical stability, high production cost of lithium cobalt oxide, and low specific energy of the battery. To achieve the effect of long service life, light weight and short charging time
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0054] A kind of high-nickel quaternary cathode material precursor, chemical formula is Ni 0.815 co 0.15 al 0.0175 mn 0.0175 (OH) 2 , its preparation method is:
[0055] Step (a), calculate and weigh soluble nickel salt, soluble cobalt salt, soluble aluminum salt and soluble manganese salt according to the molar ratio of each element Ni: Co: Al: Mn=0.815: 0.15: 0.0175: 0.0175; add them together Mix in deionized water to prepare 0.5mol / L solution A;
[0056] Step (b), adding sodium tartrate to deionized water is mixed with solution B of 0.05mol / L;
[0057] Step (c), adding sodium hydroxide to deionized water to prepare a solution C of 1mol / L;
[0058] Step (d), control the reaction temperature of the system at 40°C, add solution A, solution B and solution C into the reactor, control the stirring speed to 800 rpm, and adjust the pH of the mixed solution to 7.5, and carry out coprecipitation reaction for 3 hours Afterwards, the precipitate is filtered, washed, and dried, w...
Embodiment 2
[0060] A kind of high-nickel quaternary cathode material precursor, chemical formula is Ni 0.815 co 0.15 al 0.014 mn 0.021 (OH) 2 , its preparation method is:
[0061] Step (a), calculate and weigh soluble nickel salt, soluble cobalt salt, soluble aluminum salt and soluble manganese salt according to the molar ratio of each element Ni: Co: Al: Mn=0.815:0.15:0.014:0.021; add them together Mix in deionized water to prepare 1mol / L solution A;
[0062] Step (b), adding ammonia water to deionized water to prepare 0.2mol / L solution B;
[0063] Step (c), adding sodium hydroxide to deionized water to prepare a solution C of 2mol / L;
[0064] Step (d), control the reaction temperature of the system at 40°C, add solution A, solution B and solution C to the reactor, control the stirring speed to 750 rpm, and adjust the pH of the mixed solution to 7.0, and carry out coprecipitation reaction for 3 hours Afterwards, the precipitate is filtered, washed, and dried, wherein the drying te...
Embodiment 3
[0066] A kind of high-nickel quaternary cathode material precursor, chemical formula is Ni 0.815 co 0.15 al 0.021 mn 0.014 (OH) 2 , its preparation method is:
[0067] Step (a), calculate and weigh soluble nickel salt, soluble cobalt salt, soluble aluminum salt and soluble manganese salt according to the molar ratio of each element Ni: Co: Al: Mn = 0.815: 0.15: 0.021: 0.014; add them together Mix in deionized water to prepare 2mol / L solution A;
[0068] Step (b), adding sodium tartrate to deionized water is mixed with solution B of 0.05mol / L;
[0069] Step (c), adding potassium hydroxide to deionized water to prepare a solution C of 1mol / L;
[0070] Step (d), control the reaction temperature of the system at 40°C, add solution A, solution B and solution C into the reactor, control the stirring speed to 800 rpm, and adjust the pH of the mixed solution to 7.5, and carry out coprecipitation reaction for 3 hours Afterwards, the precipitate is filtered, washed, and dried, wh...
PUM
Property | Measurement | Unit |
---|---|---|
density | aaaaa | aaaaa |
density | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com