A kind of production method of the blanket with strong color fastness
A production method and technology for color fastness, applied in the direction of dyeing, textile material processing, knitting, etc., can solve the problems of low color fastness, unsatisfactory dyeing effect of blankets, rubbing and fading of blankets, etc., and achieve high color fastness, Avoid rubbing faded, brightly colored effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0030] A kind of production method of the blanket of strong color fastness, comprises the following steps:
[0031] (1) Warping and knitting: including three steps of warping, warp knitting and cashmere splitting, among which:
[0032] Warping: 300D / 96f polyester fiber is selected as the raw material for the veil, and 100D / 48f polyester full-drawn yarn is used as the raw material for the bottom yarn. The polyester fiber and polyester full-drawn yarn are composed of the following components: Ingredients: polyethylene terephthalate masterbatch 100g, polyvinyl chloride resin 10g, polytetrafluoroethylene resin 35g, nano fluorite powder 8g, barium hardate 1g, dicumyl peroxide 0.5g, oxidized Zinc 0.2g and silane coupling agent 1.0g;
[0033] During warping, warp at a speed of 600m / min on the H40-21NC computer-controlled copy warping machine. The yarn head is 40 inches, 48,000-50,000 meters per head, and the warp number of each head is 330. Each group The number of pan heads is 8; ...
Embodiment 2
[0072] A kind of production method of the blanket of strong color fastness, the difference with embodiment 1 is:
[0073] Step (1) Warping and weaving: the polyester fiber and polyester full-drawn yarn used are made of the following components: polyethylene terephthalate masterbatch 105g, polyvinyl chloride resin 12g, polytetrafluoroethylene resin 37g, 9g of nano-fluorite powder, 1.2g of barium stearate, 0.6g of dicumyl peroxide, 0.3g of zinc oxide and 1.2g of silane coupling agent;
[0074] The warping tension of the veil during warping is 16cN / 16.7tex, and the warping tension of the bottom yarn is 10cN / 11.11tex;
[0075] The machine warp knitting speed of warp knitting is 510 rev / min.
[0076] Step (2) white gray cloth processing:
[0077] The temperature of gray cloth when getting off the car is 52°C;
[0078] The combing speed after shaping is 17m / min; the speed of the large cylinder is 72 rpm, the parameters of the left and right brushes are 15.92m / min; the front pulli...
Embodiment 3
[0085] A kind of production method of the blanket of strong color fastness, the difference with embodiment 1 is:
[0086] Step (1) Warping and weaving: the polyester fiber and polyester full-drawn yarn used are made of the following components: polyethylene terephthalate masterbatch 110g, polyvinyl chloride resin 14g, polytetrafluoroethylene resin 40g, 10g of nano-fluorite powder, 1.6g of barium stearate, 0.8g of dicumyl peroxide, 0.4g of zinc oxide and 1.5g of silane coupling agent;
[0087] During warping, the warping tension of the veil is 18cN / 16.7tex, and the warping tension of the bottom yarn is 11cN / 11.11tex;
[0088] The machine warp knitting speed of warp knitting is 530 rev / min.
[0089] Step (2) white gray cloth processing:
[0090] The temperature of gray cloth when getting off the car is 53°C;
[0091] The combing speed after shaping is 17m / min; the rotation speed of the large cylinder is 73 rpm, the parameters of the left and right brushes are 16.92m / min; the ...