Modified calcite for purifying tetracycline in water and preparation method of modified calcite
A technology of calcite and tetracycline, applied in chemical instruments and methods, inorganic chemistry, water pollutants, etc., can solve problems such as poor adsorption effect, adverse effects on health and survival, and huge ecotoxicological effects
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0031] A modified calcite for purifying tetracycline in water and a preparation method thereof, comprising the following raw materials in parts by weight: 80 parts of calcite, 55 parts of disodium hydrogen phosphate, and 15 parts of dispersant.
[0032] The preparation method of above-mentioned modified calcite is:
[0033] (1) Calcite is washed, pulverized, and sieved to obtain calcite powder;
[0034] (2) placing 10 parts by weight of calcite powder in water, utilizing ultrasonic vibration for 40-50 hours, and taking supernatant A for subsequent use;
[0035] (3) Mix remaining calcite with supernatant A, and obtain solution A by ultrasonic vibration for 20-30 h, and adjust the pH of solution A to be 8.3;
[0036] (4) Put the solution A into the heating kettle, heat it to 160-180℃ at a speed of 2-3℃ / min, keep it warm for 20-30min, then lower it to normal temperature, and add disodium hydrogen phosphate into the heating kettle;
[0037] (5) Add the dispersion liquid into the...
Embodiment 2
[0040] A modified calcite for purifying tetracycline in water and a preparation method thereof, comprising the following raw materials in parts by weight: 90 parts of calcite, 65 parts of disodium hydrogen phosphate, and 30 parts of dispersant.
[0041] The preparation method of above-mentioned modified calcite is:
[0042] (1) Calcite is washed, pulverized, and sieved to obtain calcite powder;
[0043] (2) placing 12 parts by weight of calcite powder in water, utilizing ultrasonic vibration for 40-50 hours, and taking supernatant A for subsequent use;
[0044] (3) Mix remaining calcite with supernatant A, and obtain solution A by ultrasonic vibration for 20-30 h, and adjust the pH value of solution A to be 8.9;
[0045] (4) Put the solution A into the heating kettle, heat it to 160-180℃ at a speed of 2-3℃ / min, keep it warm for 20-30min, then lower it to normal temperature, and add disodium hydrogen phosphate into the heating kettle;
[0046] (5) Add the dispersion liquid in...
Embodiment 3
[0049] A modified calcite for purifying tetracycline in water and a preparation method thereof, comprising the following raw materials in parts by weight: 80 parts of calcite, 65 parts of disodium hydrogen phosphate, and 15 parts of dispersant.
[0050] The preparation method of above-mentioned modified calcite is:
[0051] (1) Calcite is washed, pulverized, and sieved to obtain calcite powder;
[0052] (2) placing 10 parts by weight of calcite powder in water, utilizing ultrasonic vibration for 40-50 hours, and taking supernatant A for subsequent use;
[0053](3) Mix remaining calcite with supernatant A, and obtain solution A by ultrasonic vibration for 20-30 h, and adjust the pH value of solution A to be 8.9;
[0054] (4) Put the solution A into the heating kettle, heat it to 160-180℃ at a speed of 2-3℃ / min, keep it warm for 20-30min, then lower it to normal temperature, and add disodium hydrogen phosphate into the heating kettle;
[0055] (5) Add the dispersion liquid int...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com