A feed additive and elemental sulfur technology, applied in the field of hydrotalcite-loaded elemental sulfur and its preparation, can solve problems such as disease outbreaks, cross-infection of pathogenic bacteria, economic losses of farmers, etc., and achieve inhibition of proliferation, uniform and stable dispersion, and good biophase Effects of capacitative and gastrointestinal mucosal affinity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0023] Preparation: According to "Oral Vanadium Supplement Using Bimetal Oxide as Carrier and Its Preparation and Use" (see: Ye Ying, Feng Lujia, Zheng Libo, Shen Zhongyue, Han Jie, Chen Zhifei, Li Shanshan. National Invention Patent Authorization Announcement No. The method of CN 1187091C) prepares hydrotalcite.
[0024] 1) Grind the hydrotalcite obtained in the preliminary step to 400 mesh, add water and stir to make a suspension slurry with a concentration of 10%:
[0025] 2) Sulfur content is the sodium sulfite of hydrotalcite weight 1% and the sodium sulfide that the molar ratio is 2 times of sodium sulfite, slowly add in the suspension slurry of step 1) under stirring, then add the dilute sulfuric acid that molar concentration is 0.5moL / L , adjust pH=3.0, and react at room temperature for 5 hours;
[0026] 3) centrifugal dehydration of the suspension slurry in step 2);
[0027] 4) drying and pulverizing the filter cake obtained in step 3) to 300 meshes to obtain a load...
Embodiment 2
[0029] Preparation: according to the method of "a method for preparing bimetallic oxides and hydrotalcite" (see: Ye Ying, Li Shanshan, Chen Zhifei, Zheng Libo, Huang Xia, Wu Daidai, Han Jie, Zhang Weirui. National Invention Patent Authorization Announcement No. CN 1222467C) Preparation of hydrotalcite.
[0030] 1) Grind the hydrotalcite obtained in the preliminary step to 500 mesh, add water and stir to make a suspension slurry with a concentration of 5%:
[0031] 2) Sodium bisulfite that the sulfur content is 5% by weight of hydrotalcite and the sodium sulfide that the molar ratio is 2 times of sodium bisulfite are slowly added in the suspension slurry of step 1) under stirring, and the molar concentration is 1.5 MoL / L of dilute sulfuric acid, adjust pH=5.0, and react at room temperature for 8 hours;
[0032] 3) the suspension slurry of step 2) is filtered and dehydrated;
[0033] 4) drying and pulverizing the filter cake obtained in step 3) to 400 meshes to obtain a loaded...
Embodiment 3
[0035] 1) Grind commercially available hydrotalcite to 500 mesh, add water and stir evenly to prepare a suspension slurry with a concentration of 1%:
[0036] 2) The sulfur content is the sodium sulfite heptahydrate (Na 10% by weight of hydrotalcite); 2 SO 3 ·7H 2 0) and the sodium sulfide that molar ratio is 2 times of sodium sulfite, slowly add in the suspension slurry of step 1) under stirring, then add the dilute sulfuric acid that molar concentration is 1.5moL / L, adjust pH=4.0, and react at room temperature for 10 hours;
[0037] 3) the suspension slurry of step 2) is filtered and dehydrated;
[0038]4) drying and pulverizing the filter cake obtained in step 3) to 400 meshes to obtain a loaded elemental sulfur feed additive. The content of sulfur in hydrotalcite is 10%.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com