Defoaming agent for coating material ink
A coating ink, defoamer technology, applied in the direction of ink, application, coating, etc., can solve the problems of poor dispersion of silicone, no defoaming activity, too large particle size, etc., to achieve good defoaming, improve viscosity increase, The effect of stable quality
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0018] A kind of defoamer for coating ink, in parts by mass, adopts the following steps to make:
[0019] S1, after mixing 20 parts of polydimethylsiloxane, 8 parts of higher carbon alcohol, 3 parts of zinc stearate, 1 part of methyl acrylate, 4 parts of monoglycerin fatty acid ester, and 0.5 part of secondary alkyl sodium sulfonate , and stir evenly to prepare liquid A;
[0020] S2, add 3 parts of sodium hexametaphosphate, 2 parts of sorbitan fatty acid and 3 parts of carboxymethyl cellulose into 85 parts of deionized water, and stir evenly to obtain liquid B;
[0021] S3, mix liquid A and liquid B at 70°C, heat up to 100°C and stir evenly, then add 15 parts of hydrophobic silicon dioxide and keep warm for 30 minutes to prepare a defoamer for paint and ink.
Embodiment 2
[0023] A kind of defoamer for coating ink, in parts by mass, adopts the following steps to make:
[0024] S1, mix 30 parts of polymethyltriethoxysilane, 5 parts of higher carbon alcohol, 1 part of zinc stearate, 4 parts of methyl acrylate, 2 parts of monoglyceride fatty acid ester, and 2 parts of sodium secondary alkyl sulfonate Finally, stir evenly to obtain liquid A;
[0025] S2, add 3 parts of sodium hexametaphosphate, 5 parts of polysorbate and 1.5 parts of carboxyethyl cellulose into 70 parts of deionized water, and stir evenly to prepare liquid B;
[0026] S3, mix liquid A and liquid B at 60°C, heat up to 90°C and stir evenly, add 30 parts of hydrophobic silicon dioxide and 0.1 part of tetrabutylammonium fluoride, and keep warm for 40 minutes to prepare a disinfectant for coating ink. foaming agent.
Embodiment 3
[0028] A kind of defoamer for coating ink, in parts by mass, adopts the following steps to make:
[0029] S1, after mixing 40 parts of polymethyltrimethoxysilane, 15 parts of higher alcohol, 2 parts of zinc stearate, 2 parts of methyl acrylate, 4 parts of monoglyceride fatty acid ester, and 1 part of sodium secondary alkyl sulfonate , and stir evenly to prepare liquid A;
[0030] S2, add 2 parts of sodium hexametaphosphate, 3 parts of fatty acid esters of glycerol and 2 parts of xanthan gum into 75 parts of deionized water, and stir evenly to prepare liquid B;
[0031] S3, mix liquid A and liquid B at 65°C, heat up to 95°C and stir evenly, then add 20 parts of hydrophobic silicon dioxide, 0.2 parts of tetrabutylammonium fluoride and 2 parts of glutaraldehyde, and keep warm for 35 minutes. A defoamer for coating ink is prepared.
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com