Environment-friendly internal wall paint and preparation method thereof
An interior wall coating and environmental protection technology, applied in the direction of fireproof coating, antifouling/underwater coating, coating, etc., can solve the problems of insignificant improvement effect, poor stain resistance, poor scrub resistance, etc., to achieve Difficult to stain, wide source of raw materials, and low cost
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0024] An environmentally friendly interior wall paint, the following raw materials are weighed: 30kg of styrene-acrylic emulsion, 15kg of polyvinyl alcohol resin, 10kg of silica sol, 5kg of sodium naphthenate, 8kg of polyethylene oxide, 4kg of talc powder, 5kg of modified diatom powder, Glycerin rosin resin 3kg, polyvinyl alcohol 4kg, dispersant 1kg, wetting agent 1kg, leveling agent 1kg, defoamer 1kg and film-forming aid 1kg;
[0025] The above-mentioned modified diatom powder is prepared from the following ingredients: 30kg of diatomite, 8kg of titanium dioxide, 4kg of lithopone, 3kg of lignin, 10kg of expanded perlite, 6kg of ferric chloride, and 3kg of n-butyraldehyde-aniline condensate , 3 kg of praseodymium oxide and 5 kg of beeswax; the preparation method is to soak diatomaceous earth in 8% hydrochloric acid solution for 40 minutes, dry the obtained material after suction filtration, mix with expanded perlite, and carry out high temperature at 680 ° C. Calcinate for 1 ...
Embodiment 2
[0032] An environment-friendly interior wall paint, the following raw materials are weighed: 35kg of styrene-acrylic emulsion, 20kg of polyvinyl alcohol resin, 15kg of silica sol, 10kg of sodium naphthenate, 10kg of polyethylene oxide, 8kg of talcum powder, 10kg of modified diatom powder, Glycerin rosin resin 5kg, polyvinyl alcohol 6kg, dispersant 3kg, wetting agent 3kg, leveling agent 2kg, defoamer 2kg and film-forming aid 2kg;
[0033] The above-mentioned modified diatom powder is prepared from the following ingredients: 30kg of diatomite, 8kg of titanium dioxide, 4kg of lithopone, 3kg of lignin, 10kg of expanded perlite, 6kg of ferric chloride, and 3kg of n-butyraldehyde-aniline condensate , 3 kg of praseodymium oxide and 5 kg of beeswax; the preparation method is to soak diatomaceous earth in 10% hydrochloric acid solution for 50 minutes, dry the obtained material after suction filtration, mix with expanded perlite, and carry out high temperature at 700 ° C. Calcinate for ...
Embodiment 3
[0040]An environment-friendly interior wall paint, the following raw materials are weighed: 40kg of styrene-acrylic emulsion, 25kg of polyvinyl alcohol resin, 20kg of silica sol, 15kg of sodium naphthenate, 12kg of polyethylene oxide, 12kg of talcum powder, 15kg of modified diatom powder, Glycerin rosin resin 7kg, polyvinyl alcohol 8kg, dispersant 5kg, wetting agent 5kg, leveling agent 3kg, defoamer 3kg and film-forming aid 3kg;
[0041] The above-mentioned modified diatom powder is prepared from the following ingredients: 30kg of diatomite, 8kg of titanium dioxide, 4kg of lithopone, 3kg of lignin, 10kg of expanded perlite, 6kg of ferric chloride, and 3kg of n-butyraldehyde-aniline condensate , 3 kg of praseodymium oxide and 5 kg of beeswax; the preparation method is to soak diatomite in 12% hydrochloric acid solution for 60 minutes, dry the obtained material after suction filtration, mix with expanded perlite, and carry out high temperature at 720 ° C. Calcinate for 2 hours, ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com