Aqueous and elastic thermal-insulation energy-conservation paint and preparation thereof
An elastic thermal insulation and energy-saving coating technology, used in fire-resistant coatings, coatings, etc., can solve the problems of cumbersome construction, high cost, easy cracking, etc., and achieve excellent adhesion, long service life, and good fire resistance.
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0052] A water-based elastic thermal insulation and energy-saving coating, which includes the following components in parts by weight:
[0053] Elastic emulsion 220 parts
[0054] Hollow glass powder 50 parts
[0055] 30 parts of antimony tin oxide
[0056] Titanium dioxide 50 parts
[0057] Kaolin 60 parts
[0058] Hydroxyethyl cellulose 0.8 parts
[0059] Mineral oil-based defoamer 5 parts
[0060] Sodium polyacrylate 4 parts
[0061] Ammonia water 0.8 part
[0062] Non-ionic polyether thickener 5 parts
[0063] Soft water 125 parts
[0064] The production method is as follows:
[0065] 1. Add 85% of the formula amount of soft water, formula amount of hydroxyethyl cellulose, formula amount of mineral oil-based defoamer, formula amount of sodium polyacrylate and ammonia water to the dispersing kettle, 1200 rpm, high-speed dispersion 10min.
[0066] 2. Put in the formulated amount of titanium dioxide and the formulated amount of kaolin, 1200 rpm, high-speed dispersi...
Embodiment 2
[0071] A water-based elastic thermal insulation and energy-saving coating, which includes the following components in parts by weight:
[0072] elastic emulsion 200 parts
[0073] Hollow zirconium bead powder 40 parts
[0075] Titanium dioxide 40 parts
[0076]Heavy calcium 50 parts
[0077] Methyl hydroxyethyl cellulose 0.5 part
[0078] Silicone defoamer 4 parts
[0079] 3 parts polycarboxylate sodium salt
[0080] 0.5 parts of 10% sodium hydroxide
[0081] Polyurethane comprehensive thickener 4 parts
[0082] Soft water 115 parts
[0083] The production method is as follows:
[0084] 1. Add 85% soft water, methyl hydroxyethyl cellulose, organic silicon defoamer, sodium polycarboxylate and 10% of the formula to the dispersing kettle in sequence Sodium hydroxide, 1000 rpm, high-speed dispersion for 5 minutes.
[0085] 2. Put in the formulated amount of titanium dioxide and the formulated amount of heavy calcium, 1000 rpm, high-speed d...
Embodiment 3
[0090] A water-based elastic thermal insulation and energy-saving coating, which includes the following components in parts by weight:
[0091] Elastic Lotion 250 parts
[0092] Vermiculite 60 parts
[0093] 35 parts of chromium oxide
[0094] Titanium dioxide 60 parts
[0095] Talcum powder 70 parts
[0096] Hypromellose 1.0 parts
[0097] Non-ionic defoamer 6 parts
[0098] 5 parts ammonium polyacrylate
[0099] 2 amino-2 methyl-propanol 1.0 parts
[0100] Alkali swelling thickener 6 parts
[0101] Soft water 135 parts
[0102] The production method is as follows:
[0103] 1. Add 85% soft water of formula quantity, hydroxypropyl cellulose of formula quantity, nonionic defoamer of formula quantity, polyacrylic acid ammonium salt of formula quantity and 2 amino-2 methyl- Propanol, 1200 rpm, high-speed dispersion for 8 minutes.
[0104] 2. Put in the formula amount of titanium dioxide and talc powder, 1200 rpm, high-speed dispersion for 25 minutes, then transfer to t...
PUM
Property | Measurement | Unit |
---|---|---|
Thermal conductivity | aaaaa | aaaaa |
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com