Anti-fouling wear-resisting transparent fluorine-silicone polymer material and preparation method thereof

A polymer material, transparent technology, applied in antifouling/underwater coatings, coatings, paints containing biocides, etc., can solve problems such as corrosion, low product performance, pollution of equipment, etc., to avoid environmental pollution and improve product quality. performance, the effect of reducing production costs

Inactive Publication Date: 2013-02-06
XIAMEN MINGDA TECH
View PDF6 Cites 15 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

[0006] At present, the production of fluorosilicon materials has spread all over the country, but the friction resistance of domestically produced fluorosilicon products is relatively low. After a certain degree of wear, the waterproof and oil-proof performance is seriously reduced; The contact angle of the hydrophobic coating to water will decrease with the prolongation of outdoor use time, and the hydrophobicity will decrease
This is mainly caused by the adsorption and accumulation of dust and organic pollutants in the air on the solid surface; most of the existing antifouling fluorosilicon polymer materials are produced by indirect methods, because there are many intermediate products, the synthesis route is complicated, and the products are not easy to purify. And the purpose is single, the enterprise device is a closed chain, so there are more prominent pollution and equipment corrosion problems, the cost is relatively high, and the product performance is low
With the rapid development of the market and the tightening of environmental protection policies, the existing anti-fouling fluorosilicon polymer materials can no longer adapt to the development of fluorosilicon polymer materials.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Anti-fouling wear-resisting transparent fluorine-silicone polymer material and preparation method thereof
  • Anti-fouling wear-resisting transparent fluorine-silicone polymer material and preparation method thereof
  • Anti-fouling wear-resisting transparent fluorine-silicone polymer material and preparation method thereof

Examples

Experimental program
Comparison scheme
Effect test

Embodiment 1

[0033] Example 1 Preparation of anti-fouling and wear-resistant transparent fluorosilicone polymer material

[0034] Add 10 grams of 1-iodoperfluorooctane, 20 grams of vinyl triisopropoxy silane, 100 grams of methanol, 0.05 grams of initiator ammonium persulfate, and fungicide tetradecyl dimethyl into the high pressure reactor. Benzyl ammonium chloride 0.001 grams, additives nano titanium dioxide powder 0.005 grams. Seal the autoclave and fill it with nitrogen until the pressure reaches 2 atmospheres. Start heating. When heated to 90°C, constant-temperature polymerization starts at a stirring speed of 500 revolutions per minute. After 12 hours, the polymerization reaction is stopped and quickly cooled to room temperature. The target product can be obtained by removing the solvent from the product.

Embodiment 2

[0035] Example 2 Preparation of anti-fouling and wear-resistant transparent fluorosilicone polymer material

[0036] Add 20 grams of perfluorooctyl ethylene, 30 grams of vinyl tri-tert-butoxy silane, 100 grams of ethanol, 0.4 grams of initiator potassium persulfate, and 0.02 grams of bactericide pentachloronitrobenzene into the autoclave. 0.1 g of nanometer titanium dioxide powder. Seal the autoclave and fill it with nitrogen until the pressure reaches 5 atmospheres. Start heating. When heated to 120°C, constant temperature polymerization starts at a stirring speed of 900 revolutions per minute. After 12 hours, the polymerization reaction is stopped and quickly cooled to room temperature. The target product can be obtained by removing the solvent from the product.

Embodiment 3

[0037] Example 3 Preparation of anti-fouling and wear-resistant transparent fluorosilicone polymer material

[0038] Add 15 grams of allyl perfluoroether, 25 grams of vinyl trimethoxysilane, 100 grams of propanol, 0.2 grams of initiator sodium persulfate, and 0.01 grams of bactericide tetrachloroisophthalonitrile into the autoclave. Additives: 0.05 grams of nano titanium dioxide powder. Seal the autoclave and fill it with nitrogen until the pressure reaches 3 atmospheres. Start heating. When heated to 100°C, constant-temperature polymerization starts at 700 revolutions per minute. The polymerization reaction is stopped after 12 hours and quickly cooled to room temperature. The target product can be obtained by removing the solvent from the product.

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

No PUM Login to view more

Abstract

The invention relates to an anti-fouling wear-resisting transparent fluorine-silicone polymer material and a preparation method thereof. The fluorine-silicone polymer material contains perfluoroalkyl and silicon-oxygen alkyl. The preparation method comprises the steps of adding an unsaturated monomer containing fluorine, an unsaturated siloxane monomer, a reaction solvent, an initiator, auxiliaries and bactericide into a high pressure reactor; and under the protection of nitrogen, heating and warming, controlling the pressure of the reactor, adjusting stirring, carrying out constant-temperature stirring reaction for 8-16 hours, and then fast cooling to room temperature. The fluorine-silicone polymer material can be coated on the surface of substrates such as glass, metal, plastic and the like in modes of spray coating, roll coating, wiping and the like to achieve the effectively waterproof, oil-proof, anti-fouling and wear-resisting effects.

Description

Technical field [0001] The invention relates to a transparent fluorosilicon polymer material with hydrophobic, oleophobic, antifouling, abrasion resistance and other properties and a preparation method thereof, belonging to the field of functional polymer materials. Background technique [0002] In recent years, the R&D and industrialization of new polymer functional materials in our country have developed rapidly. The national industrial policy encourages the development of new polymer functional materials industry towards high-tech products. The development of the fluorosilicone polymer materials industry and other related industries, especially the foundation The chemical industry is closely related to the infrastructure industry, and the rapid development of the fluorosilicon industry will forcefully promote the sound and rapid development of the basic chemical industry and infrastructure industry. [0003] In recent years, the preparation of hydrophobic, oleophobic, antifoulin...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(China)
IPC IPC(8): C08F230/08C08F214/18C08F216/14C08F228/02C08F2/22C08K3/22C09D143/04C09D5/16C09D7/12
Inventor 查选义
Owner XIAMEN MINGDA TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products