Industrial wastewater treating agent
A technology for industrial wastewater and treatment agents, applied in water/sewage treatment, adsorption water/sewage treatment, biological water/sewage treatment, etc., can solve the problems of reduced drug efficacy, large dosage of chemicals, high cost, etc., and achieve chemical Stable properties, low processing cost, and good adsorption capacity
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0019] An industrial wastewater treatment agent, which is mainly made of the following raw materials in parts by weight: 20 parts of polysilicon aluminum sulfate, 23 parts of ferric sulfate, 3 parts of polyacrylamide, 4 parts of microorganisms, 22 parts of potato starch, polyethylene 8 parts of amine, 11 parts of alum, 7 parts of tannin, 8 parts of sodium tripolyphosphate, 30 parts of modified volcanic stone, 15 parts of calcium hydroxide, 15 parts of activated carbon, 9 parts of potassium persulfate, 3 parts of sodium acetate and lignin 10 servings.
[0020] The preparation method of described modified volcanic stone is as follows:
[0021] (1) pretreatment of the volcanic stone, drying the volcanic stone at a temperature of 90-100°C for 15 hours; then calcining the volcanic stone at a temperature of 550-600°C for 2.5 hours;
[0022] (2) Modification of volcanic stone: after the volcanic stone after step (1) is calcined is cooled, add volcanic stone to 40% sulfuric acid solu...
Embodiment 2
[0029] An industrial wastewater treatment agent, which is mainly made of the following raw materials in parts by weight: 15 parts of polysilicon aluminum sulfate, 30 parts of ferric sulfate, 1 part of polyacrylamide, 5 parts of microorganisms, 15 parts of potato starch, polyethylene 3 parts of amine, 7 parts of alum, 10 parts of tannin, 4 parts of sodium tripolyphosphate, 40 parts of modified volcanic stone, 10 parts of calcium hydroxide, 20 parts of activated carbon, 5 parts of potassium persulfate, 1 part of sodium acetate and lignin 5 servings.
[0030] The preparation method of described modified volcanic stone is as follows:
[0031] (1) pretreatment of the volcanic stone, drying the volcanic stone at a temperature of 90-100°C for 20 hours; then calcining the volcanic stone at a temperature of 550-600°C for 2 hours;
[0032] (2) Modification of volcanic stone: After the volcanic stone after the calcining in step (1) is cooled, add volcanic stone to 40% sulfuric acid solu...
Embodiment 3
[0039] An industrial wastewater treatment agent, which is mainly made of the following raw materials in parts by weight: 30 parts of polysilicon aluminum sulfate, 15 parts of ferric sulfate, 5 parts of polyacrylamide, 1 part of microorganism, 30 parts of potato starch, polyethylene 13 parts of amine, 17 parts of alum, 5 parts of tannin, 11 parts of sodium tripolyphosphate, 20 parts of modified volcanic stone, 20 parts of calcium hydroxide, 10 parts of activated carbon, 15 parts of potassium persulfate, 5 parts of sodium acetate and lignin 20 servings.
[0040] The preparation method of described modified volcanic stone is as follows:
[0041] (1) pretreatment of the volcanic stone, drying the volcanic stone at a temperature of 90-100°C for 10 hours; then calcining the volcanic stone at a temperature of 550-600°C for 3 hours;
[0042] (2) Modification of volcanic stone: after the volcanic stone after the calcining of step (1) is cooled, add volcanic stone to 40% sulfuric acid ...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com