Surface alloying ceramic and its preparing process

A technology for surface alloying and ceramic preparation, applied in the field of surface alloying ceramics and preparation, can solve the problems of easy cracking, decreased ceramic surface finish, poor adaptability, etc., to reduce the interface stress concentration, avoid obstruction and embrittlement Influence and improve the effect of interface bonding strength

Inactive Publication Date: 2007-02-14
TAIYUAN UNIV OF TECH
View PDF4 Cites 0 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Problems solved by technology

The Mn-Mo method is to sinter Mn and Mo powder materials on the ceramic surface during the complex sintering process. This metallization process reduces the surface finish and performance of the ceramics; the vapor deposition metallization method is characterized by ceramics that do not withstand high temperatures. , can ensure the dimensional accuracy of the parts, the metallized film is continuous and dense, has good thermal conductivity, low high-frequency loss, and high strength, but it can only deposit a single metal element, so it can only be called a ceramic surface metallization method. In addition, because it has no activity The role of elements, the bonding strength of the metal layer and ceramics is low
[0005] Based on the beneficial effect of the chemical reaction between active element titanium and ceramics, the applicant has carried out arc glow titanium infiltration on the ceramic surface, but this method only makes the ceramic surface realize titanium metallization, the metal element is single, and the adaptability is poor , and due to the strong oxygen affinity of titanium, the metal titanium layer is easily oxidized by the atmosphere, and the formation of an oxide film is not conducive to the subsequent application process
For example, in the connection between ceramics and metals based on this, since the titanium layer permeated on the surface of the ceramics is difficult to react and mix with the solder during the brazing process, a layer of titanium is retained on the ceramic side of the ceramics and metal connection joints. layer, which affects the wetting and reaction of the solder and the ceramic, and directly affects the connection strength between the ceramic and the metal. The presence of a large number of intermetallic compounds on the ceramic side of the joint increases the brittleness of the joint, and it is prone to cracking under the action of residual stress

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Surface alloying ceramic and its preparing process
  • Surface alloying ceramic and its preparing process
  • Surface alloying ceramic and its preparing process

Examples

Experimental program
Comparison scheme
Effect test

Embodiment approach 1

[0027] Surface alloyed Al 2 o 3 Preparation of ceramics for the purpose of conducting surfaces.

[0028] Ceramic is Al 2 o 3 , The composite target adopts three components of titanium, copper, and aluminum, and is arranged as copper, aluminum, and titanium materials from outside to inside, and the area ratio is 30-40%, 30-40%, and 20-40%. The process parameters of ceramic surface alloying are:

[0029] Ultimate vacuum 6Pa Glow voltage 600V

[0030] Arc current 60A Dipping time 30min

[0031] Working medium argon

[0032] Al 2 o 3 The thickness of the alloy layer on the ceramic surface is 20 μm, which has good electrical conductivity.

Embodiment approach 2

[0034] Surface Alloyed Ceramics for Microjoints

[0035] The ceramic material is Al 2 o 3 , the metal is aluminum foil after 15 μm, the composite target adopts two components of aluminum and titanium, aluminum is used as the outer ring, titanium is used as the inner ring, and the area ratio of aluminum and titanium in the composite target is 60-80% and 20-40%. The surface alloyed ceramics are connected with metal and solder in a vacuum furnace.

[0036] The process parameters of ceramic surface alloying and brazing with metal are:

[0037] Ultimate vacuum 6Pa Working air pressure 20Pa

[0038] Glow voltage 700V Arc current 60A

[0039] Dipping time 50min Brazing temperature 500℃

[0040] Holding time 10min Working medium Argon

[0041] Al2 o 3 The thickness of the infiltrated alloy layer on the ceramic surface is 10-20 μm, and the brazing results show that Al 2 o 3 The ceramic / metal aluminum foil joint has no cracks, and the entire joint surface has no unconnected pla...

Embodiment approach 3

[0043] Low vacuum brazing of surface alloyed ceramics to metals for ceramic / metal joints

[0044] The ceramic material is Si 3 N 4 , the metal material is carbon steel Q235, the composite target uses copper, titanium and iron three components, copper is used as the outer ring, titanium copper is used as the inner ring, and the area ratio of copper, titanium and iron is 40-60%, 20-40% , 10-40%, the surface alloyed ceramics and metals and Ag-Cu solder are placed in a vacuum furnace for brazing.

[0045] The process parameters of ceramic surface alloying and brazing with metal are:

[0046] Ultimate vacuum 6Pa Working air pressure 20Pa

[0047] Glow voltage 700V Arc current 60A

[0048] Dipping time 50min Brazing temperature 850℃

[0049] Brazing vacuum 5×10 -2 Pa holding time 10min

[0050] Working medium argon

[0051] The thickness of the alloy layer on the ceramic surface is 30μm, the quality of the brazed joint is good, Si 3 N 4 The ceramic has no cracks, and the e...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

PUM

PropertyMeasurementUnit
thicknessaaaaaaaaaa
thicknessaaaaaaaaaa
shear strengthaaaaaaaaaa
Login to View More

Abstract

This invention discloses a surface alloying ceramics and its preparation method. It relates to fields of improving technology of ceramics surface and composite material preparation. The features are that common ceramics are surface alloyed in arc glowing furnace by using composite target designed by this invention method. The target is pro rate mechanic consisted by one kind or several kinds of titanium (or zirconium, hafnium) and other metal materials (such as iron, chromium, nickel, manganese, molybdenum, copper, aluminum, argentums). The target evaporates or melts under the action of the arc heat and the ceramics surface is impacted by metal ions in high speed under the action of high electric field. The advantage is that the cementation speed is fast, the bond strength is high, and the thickness of alloy layer can reach more than 100 mu m. The preparations of several kinds of surface alloying ceramics and sill like composite material can be realized by this method.

Description

1. Technical field [0001] Surface alloyed ceramics and preparation method of the present invention relate to ceramic surface modification technology and preparation of composite materials [0002] technology field. 2. Background technology [0003] Ceramic materials have many advantages, such as high temperature resistance, corrosion resistance, high hardness, wear resistance, and good electrical insulation. Therefore, ceramic materials have been widely used. However, due to the inevitable disadvantages of ceramics, such as brittleness, strength dispersion and poor processability, the further use of ceramics is limited. Alloying the surface of ceramics to form surface alloyed ceramics is the main way to maximize the strengths and avoid weaknesses to expand the application of ceramics. Therefore, surface alloyed ceramics have broad application prospects. [0004] The biggest difficulty in metallizing ceramic surfaces is that the bonding mechanism of ceramic materials and m...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to View More

Application Information

Patent Timeline
no application Login to View More
Patent Type & Authority Patents(China)
IPC IPC(8): C04B41/88
Inventor 王文先张红霞崔泽琴马丽莉
Owner TAIYUAN UNIV OF TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Patsnap Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Patsnap Eureka Blog
Learn More
PatSnap group products