Coal combustion-supporting hydrogel as well as preparation method and application thereof
A hydrogel and coal technology, applied in the field of coal combustion additives, can solve the problems of heavy metals and radioactive substances new pollution, solid particle additives are not conducive to dispersion, coke cleaning, corrosion inhibition effect is not ideal, etc., to reduce the number of fly ash , Fly ash reduction, and the effect of reducing pollutant emissions
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Examples
Embodiment 1
[0054] A coal combustion-supporting hydrogel prepared by the following steps:
[0055] (1) Mix the ingredients in the following mass percentages evenly to obtain a mixture:
[0056] Calcium nitrate: 32%
[0057] Sodium nitrate: 20%
[0058] Manganese nitrate: 15%
[0059] Potassium chlorate: 15%
[0060] Lanthanum nitrate: 3%
[0061] Sodium hydroxide: 10%
[0062] Sodium silicate: 5%;
[0063] (2) Dissolve 3% poly-N-isopropylacrylamide and 30% hydrogen peroxide in water, and stir evenly to obtain a solvent; the percentage is the percentage of the total volume of the solvent;
[0064] (3) Dissolve the mixture in a solvent to form a coal combustion-supporting hydrogel with a solid content of 30%.
[0065] The coal combustion-supporting hydrogel of this embodiment is mixed with low-quality coal at a mass ratio of 1:200 and then burned. It is used for unqualified first-class bituminous coal (below 2000 kcal / kg), such as coal mixed with a large amount of coal gangue or The...
Embodiment 2
[0068] A coal combustion-supporting hydrogel prepared by the following steps:
[0069] (1) Mix the ingredients in the following mass percentages evenly to obtain a mixture:
[0070] Calcium nitrate: 32%
[0071] Sodium nitrate: 17%
[0072] Manganese nitrate: 30%
[0073] Potassium chlorate: 10%
[0074] Cerium nitrate: 1%
[0075] Sodium hydroxide: 5%
[0076] Sodium silicate: 5%;
[0077] (2) Dissolve 3% poly-N-isopropylacrylamide and 30% hydrogen peroxide in water, and stir evenly to obtain a solvent; the percentage is the percentage of the total volume of the solvent;
[0078] (3) Dissolve the mixture in a solvent to form a coal combustion-supporting hydrogel with a solid content of 30%.
[0079] The coal combustion-supporting hydrogel of this embodiment is mixed with low-quality coal at a mass ratio of 1:200 and then burned. It is used for unqualified first-class bituminous coal (below 2000 kcal / kg), such as coal mixed with a large amount of coal gangue or The non...
Embodiment 3
[0082] A coal combustion-supporting hydrogel prepared by the following steps:
[0083] (1) Mix the ingredients in the following mass percentages evenly to obtain a mixture:
[0084] Calcium nitrate: 37%
[0085] Sodium nitrate: 38%
[0086] Potassium chlorate: 10%
[0087] Cerium nitrate: 2%
[0088] Sodium hydroxide: 5%
[0089] Sodium silicate: 8%;
[0090] (2) Dissolve 3% poly-N-isopropylacrylamide and 30% hydrogen peroxide in water, and stir evenly to obtain a solvent; the percentage is the percentage of the total volume of the solvent;
[0091] (3) Dissolve the mixture in a solvent to form a coal combustion-supporting hydrogel with a solid content of 30%.
[0092] The coal combustion-supporting hydrogel of this embodiment is mixed with low-quality coal at a mass ratio of 1:200 and then burned. It is used for unqualified first-class bituminous coal (below 2000 kcal / kg), such as coal mixed with a large amount of coal gangue or The non-combustible waste coal accumulat...
PUM
Abstract
Description
Claims
Application Information
- R&D Engineer
- R&D Manager
- IP Professional
- Industry Leading Data Capabilities
- Powerful AI technology
- Patent DNA Extraction
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2024 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com