Skeletal iron catalyst having improved attrition resistance and product selectivity in slurry-phase synthesis processes

a technology of skeletal iron and slurry, which is applied in the direction of hydrocarbon preparation, liquid hydrocarbon mixture production, oxygen-containing compound preparation, etc., can solve the problems of affecting the commercial use of the process, affecting the product quality of the reaction product, and affecting the product selectivity, so as to achieve good particle strength and attrition resistance, the catalyst recovers quickly, and the yield is high.

Inactive Publication Date: 2002-05-02
HYDROCARBON TECH
View PDF0 Cites 16 Cited by
  • Summary
  • Abstract
  • Description
  • Claims
  • Application Information

AI Technical Summary

Benefits of technology

[0008] The preparation method and treatment procedures for this skeletal iron catalyst are relatively simple and inexpensive. This resulting skeletal iron catalyst has good particle strength and attrition resistance, and activity equivalent to that of precipitated iron catalyst because during reactions its skeletal structure is easily accessible to H.sub.2 and produces larger yields of gasoline-diesel fuel range hydrocarbons and variable amounts of wax products. Also in F-T synthesis process it is easier to separate the skeletal iron catalyst from the reactor liquid medium and product, and thus achieves high recovery of the catalyst and thereby provides light hydrocarbon liquid products containing low concentrations of undesired catalyst fines.

Problems solved by technology

However, precipitated iron catalysts are undesirably fragile and break down easily under reaction conditions into very fine particles, so that separation of such fine catalyst particles from reaction product waxes is difficult to accomplish and results in inferior product quality and significant catalyst loss.
Such catalyst problems hinders commercial use of the process.
), thus requiring costly construction materials and consuming huge amounts of energy for feedstream heating and reaction.

Method used

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
View more

Image

Smart Image Click on the blue labels to locate them in the text.
Viewing Examples
Smart Image
  • Skeletal iron catalyst having improved attrition resistance and product selectivity in slurry-phase synthesis processes

Examples

Experimental program
Comparison scheme
Effect test

example 1

[0025] Mix powders iron, aluminum and a small amount of copper promotor metal powder in a respective weight proportion of 33:66:1 in an electric induction furnace, heat and melt the metal powders to form an iron metal alloy, then cool it to room temperature and pulverize the resulting iron alloy to 0.1-1.0 mm size precursor particles. Then provide a desired amount of 25% NaOH caustic solution in a stirred container, add the iron alloy precursor particles under hydrogen flow, into the caustic solution maintained at 85.degree. C. temperature, and allow reaction to proceed for 30 minutes to extract and / or leach substantially the aluminum from the iron alloy particles. Wash the particles with deionized water to pH=7, displace water with water-free ethanol and store the resulting skeletal iron catalyst particles in ethanol.

[0026] Before being evaluated in a reaction system, the ethanol-containing skeletal iron catalyst is dried and reduced under high space velocity hydrogen at 300.degree...

example 2

[0027] Mix powders iron and aluminum together with a small amount of copper promoter metal powder in weight proportion 33:66:1 into electric induction furnace, heat and melt the powders to form iron metal alloy, then cool it to room temperature and pulverize the iron alloy to 0.1-1.0 mm size precursor particles as for Example 1. Then provide a desired amount of 25% concentration NaOH in a stirred container under hydrogen stream, add the Fe-Al alloy particles into the NaOH caustic solution maintained at 75.degree. C. temperature, allow reaction for 30 minutes to extract and / or leach substantially aluminum from the iron alloy particles. Then wash the particles with de-ionized water to pH=7, displace water with water-free ethanol and store skeletal iron catalyst particles in ethanol.

[0028] Next dry and reduce the ethanol-containing skeletal iron catalyst at 300.degree. C. under high space velocity hydrogen for 2 hours, and then transfer the catalyst into liquid reaction medium (liquid ...

example 3

[0029] Mix iron and aluminum powders together with a small amount of copper promoter powder in weight ratio of 33:66:1 in an electric induction furnace, heat and melt the metal powders to form an iron-aluminum alloy, then cool to room temperature and pulverize to 0.1-1.0 mm precursor particle size same as for Example 1. Then add desired amount of 25% concentration NaOH caustic solution to a stirred container, add the Fe-Al alloy particles to the caustic solution maintained at 65.degree. C. temperature, and allow reaction for 30 minutes to extract and / or leach substantially the aluminum from the iron alloy particles. Then wash the particles with de-ionized water to pH=7, displace water with water-free ethanol, and store the resulting skeletal iron catalyst in ethanol.

[0030] Before the skeletal iron catalyst is evaluated in a reactor system, the ethanol-containing catalyst is dried and reduced at 300.degree. C. under high space velocity H.sub.2 for 2 hours, and is then transferred int...

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

PUM

PropertyMeasurementUnit
pore diameteraaaaaaaaaa
particle sizeaaaaaaaaaa
particle sizeaaaaaaaaaa
Login to view more

Abstract

Particulate skeletal iron catalyst is provided which contain at least about 50 wt. % iron with the remainder being a minor portion of a suitable non-ferrous metal and having characteristics of 0.062-1.0 mm particle size (62-1000 micron), 20-100 m2 / g surface area, and 10-40 nm average pore diameter. Such skeletal iron catalysts are prepared and utilized for producing synthetic hydrocarbon products from CO and H2 feeds by Fischer-Tropsch synthesis process. Iron powder is mixed with non-ferrous metal powder selected from aluminum, antimony, silicon, tin or zinc powder to provide 20-80 wt. % initial iron content and melted together to form an iron alloy, then cooled to room temperature and pulverized to provide 0.1-10 mm iron alloy catalyst precursor particles. The iron alloy precursor particles are treated with NaOH or KOH caustic solution at 30-95° C. temperature to extract and / or leach out most of the non-ferrous metal portion, and then screened and treated by drying and reducing with hydrogen so as to provide smaller sized skeletal iron catalyst material. Such skeletal iron catalyst is utilized with CO+H2 feedstream for Fischer-Tropsch reactions in either a fixed bed or slurry bed type reactor at 180-500° C. temperature, 0.5-5.0 mPa pressure, and gas hourly space velocity of 0.5-3.0 L / g Fe / hr to produce desired hydrocarbon products.

Description

BACKGROUND OF INVENTION[0001] This invention pertains to skeletal iron catalyst and its preparation and use in Fischer-Tropsch and similar slurry-phase synthesis processes. More particularly, such skeletal iron catalyst utilized in slurry phase synthesis processes for H.sub.2+CO feedstreams has increased attrition resistance and improved catalyst / product liquid separation, while providing increased selectivity for producing C.sub.2-C.sub.5 light olefin products.[0002] Slurry phase Fischer-Tropsch (F-T) synthesis process technology is an important known route for indirect coal liquefaction for synthesis of liquid fuels from H.sub.2+CO feedstreams. Precipitated iron is currently a commonly used catalyst for such Fischer-Tropsch processes. However, precipitated iron catalysts are undesirably fragile and break down easily under reaction conditions into very fine particles, so that separation of such fine catalyst particles from reaction product waxes is difficult to accomplish and resul...

Claims

the structure of the environmentally friendly knitted fabric provided by the present invention; figure 2 Flow chart of the yarn wrapping machine for environmentally friendly knitted fabrics and storage devices; image 3 Is the parameter map of the yarn covering machine
Login to view more

Application Information

Patent Timeline
no application Login to view more
Patent Type & Authority Applications(United States)
IPC IPC(8): B01J23/745B01J25/00B01J37/00B01J37/06B22F9/16C07C1/04C10G2/00C22C30/00C22C38/06C22C38/16
CPCB01J23/745B01J25/00B01J37/0018B01J37/06B22F9/16C22C38/16C07C2523/745C10G2/332C22C30/00C22C38/06C07C1/0445
Inventor ZHOU, PEIZHENGLEE, LAP-KEUNGZHOU, JINGLAILU, YIJUNLI, GUOHUI
Owner HYDROCARBON TECH
Who we serve
  • R&D Engineer
  • R&D Manager
  • IP Professional
Why Eureka
  • Industry Leading Data Capabilities
  • Powerful AI technology
  • Patent DNA Extraction
Social media
Try Eureka
PatSnap group products