A technology of hydroxyethyl starch and hydroxyethyl, which is applied in the field of sanitary materials, can solve the problems of inability to effectively protect the wound surface, inability to absorb rapidly, and inability to form a colloidal protective layer, so as to facilitate wound healing, avoid adhesive intestinal obstruction, The effect of promoting increased gastrointestinal motility
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0069] Weigh hydroxyethyl starch, sodium alginate, and calcium chloride according to Table 1. The molecular weight of hydroxyethyl starch is 135,000 Da, the molecular weight of sodium alginate is 6000 Da, and the G / M ratio is 1.50. Sodium alginate and hydroxyethyl starch The particle size of the fluidized granulator is 60 mesh; put the above raw materials into the fluidized granulator preheated to 70°C, start the fan of the fluidized granulator, and control the wind speed of the fluidized granulator to 25HZ, so that the material is in a fluidized state.
[0070] Table 1
[0071] Numbering
[0072] Add 100g of deionized water to the boiling granulator through the spray gun for granulation, control the motor speed when the spray gun sprays to 200rpm, the pressure is 0.2MPa, and control the wind speed of the boiling granulator to 25HZ, so that hydroxyethyl starch, sodium alginate, Calcium chloride and water are mixed and granulated, the inlet temperature of the granulat...
Embodiment 2
[0074] Weigh 500g of hydroxyethyl starch, 1000g of water-soluble chitosan, the pH of 1% aqueous solution of water-soluble chitosan is 6.5, the degree of deacetylation is 95%, the molecular weight of hydroxyethyl starch is 280,000 Da, add it to preheat to 70°C In the fluidized granulator, start the fan of the fluidized granulator, and control the wind speed of the fluidized granulator to 75HZ to make the material in a fluidized state.
[0075] Add 100g of deionized water to the boiling granulator through the spray gun for granulation, control the motor speed of the spray gun to 200rpm, the pressure 0.2MPa, and control the wind speed of the boiling granulator to 75HZ to make hydroxyethyl starch and water-soluble chitosan Sugar and water are mixed and granulated, the inlet temperature of the granulator is controlled at 90°C, the outlet temperature is 50°C, and the boiling granulation time is 2 minutes.
[0076]Packing and sealing the granulated wound dressing. Put the wound dres...
Embodiment 3
[0078] Weigh 1000g of absorbable oxidized cellulose, 5000g of hydroxyethyl starch, and 100g of β-glucan into the boiling granulator preheated to 70°C. The degree of polymerization of absorbable oxidized cellulose is 400, and the degree of polymerization of absorbable oxidized cellulose The carboxyl content in the mixture is 22%, and the molecular weight of hydroxyethyl starch is 500,000 Da; start the fan of the boiling granulator, and control the wind speed of the boiling granulator to 60HZ, so that the material is in a fluidized state.
[0079] Add 1000g of deionized water to the boiling granulator through the spray gun for granulation, control the motor speed of the spray gun to 200rpm, the pressure 0.2MPa, and control the wind speed of the boiling granulator to 60HZ, so that hydroxyethyl starch and oxidized fiber can be absorbed Vegetables, β-glucan and water were mixed and granulated, the inlet temperature of the granulator was controlled at 74°C, the outlet temperature was...
PUM
| Property | Measurement | Unit |
|---|---|---|
| molecular weight | aaaaa | aaaaa |
| particle diameter | aaaaa | aaaaa |
| specific surface area | aaaaa | aaaaa |