Antibacterial medical coated non-woven fabric and preparation method thereof
A non-woven and coating technology, applied in pharmaceutical formulations, pharmaceutical sciences, fiber types, etc., can solve the problems of incomplete wound dressing, waste of drug dressings, easy torn wounds, etc. secondary tear, reducing the risk of infection
- Summary
- Abstract
- Description
- Claims
- Application Information
AI Technical Summary
Problems solved by technology
Method used
Image
Examples
Embodiment 1
[0053] (1) Preparation of non-woven fabric:
[0054] A. Preparation of modified crystal should: mix the nano-zinc oxide whiskers, nano-titanium dioxide crystals, mix well, add a silane coupling agent, adjusting the pH of 4, and continuing to stir 30 min, resulting in modified crystal must;
[0055] B. Preparation of nonwoven fabric: N, N-dimethylformamide is added to the spinning liquid to stir mix, increase the rotational speed to 1100R / min and add modified crystal, electrostatic spinning to obtain a modified yarn, The modified yarn is made into non-woven fabric a;
[0056] C. Preparation of non-woven fabric:
[0057] a) Soak the nonwoven fabric in ethanol in ethanol, under 20 ° C, add a sodium hydroxide solution, continued to be stirred for 10 min, and then dried to obtain a nonwoven fabric B;
[0058] b) Place the sodium hydroxide in the chloroacetic acid solution to stir well, then add acrylic acid, dibenylketone stir well, adjust the pH of 6, then add nonwoven fabric a soak...
Embodiment 2
[0076] (1) Preparation of non-woven fabric:
[0077] A. Preparation modified crystal should: mix the nano-zinc oxide whiskers, nano-titanium dioxide crystals, mixed into the ethanol solution, add the silane coupling agent, adjust the pH of 5, and continue to stir 40 min, resulting in modified crystal must;
[0078] B. Preparation of nonwoven fabric: N, N-dimethylformamide is added to the spinning liquid and mix, increase the rotational speed to 1200R / min and add modified crystal, electrospinning to obtain a modified yarn, The modified yarn is made into non-woven fabric a;
[0079] C. Preparation of non-woven fabric:
[0080] a) Soak the non-woven fabric for 20 min in ethanol, under 24 ° C, add sodium hydroxide solution, continued to stir 15 min, remove the drying, to obtain a nonwoven fabric B;
[0081] b) Place the sodium hydroxide in the chloroacetic acid solution to stir well, then add acrylic acid, dibenzone stirring, adjust the pH of 7, then add nonwoven fabric a soaking 1....
Embodiment 3
[0099] (1) Preparation of non-woven fabric:
[0100] A. Preparation of modified crystal should: mix the nano-zinc oxide whiskers, nano-titanium dioxide crystals, mix well, add a silane coupling agent, adjusting the pH of 6, continued to stir 60 min, resulting in modified crystal must;
[0101] B. Preparation of non-woven fabric: N, N-dimethylformamide is added to the spinning liquid and mix, increase the rotational speed to 1300 r / min and add modified crystal, electrostatic spinning to obtain a modified yarn, The modified yarn is made into non-woven fabric a;
[0102] C. Preparation of non-woven fabric:
[0103] a) Soaked the nonwoven fabric in ethanol to 25 min, under 28 ° C, add a sodium hydroxide solution, continued to stir 20 min, and dry it to obtain a nonwoven fabric B;
[0104] b) Place the sodium hydroxide in the chloroacetic acid solution to stir well, then add acrylic acid, dibenylketone stir well, adjust the pH of 8, then add nonwoven fabric a soaking 2H, remove, ethan...
PUM
Login to View More Abstract
Description
Claims
Application Information
Login to View More - R&D
- Intellectual Property
- Life Sciences
- Materials
- Tech Scout
- Unparalleled Data Quality
- Higher Quality Content
- 60% Fewer Hallucinations
Browse by: Latest US Patents, China's latest patents, Technical Efficacy Thesaurus, Application Domain, Technology Topic, Popular Technical Reports.
© 2025 PatSnap. All rights reserved.Legal|Privacy policy|Modern Slavery Act Transparency Statement|Sitemap|About US| Contact US: help@patsnap.com